Copper Alloys dealers in UAE

C18150 / CuCr1Zr / 2.1293 Chromium Zirconium Copper | Supplier in UAE & GCC

C18150 (CuCr1Zr) — chromium zirconium copper: 420–470 MPa strength, ~80% IACS, higher softening resistance; RWMA Class 2 electrode alloy for coated steels.

Industries Served

Automotive
Manufacturing
Power Generation
Heavy Engineering
Construction
Mould & Die

Overview

C18150 chromium zirconium copper (CuCr1Zr, EN CW106C, DIN 2.1293, UNS C18150, RWMA Class 2 / ISO 5182 A2/2) is a precipitation-hardening high-copper alloy containing 0.5–1.2% chromium and 0.03–0.3% zirconium, supplied to EN 12163 for rod and to the RWMA Class 2 electrode classification. Like chromium copper it is solution treated at 982–1010°C, water quenched, cold drawn and aged at about 425–500°C, precipitating fine chromium particles that raise tensile strength to 470 MPa minimum (R470, up to 25 mm) and 420 MPa minimum (R420, 25–50 mm) while restoring conductivity to about 80% IACS. The zirconium addition forms its own fine precipitates and segregates to grain boundaries, raising the softening temperature and improving creep resistance and hot ductility, so electrode faces hold their shape longer and resist sticking when welding galvanised and coated steels. These properties make CuCrZr the preferred Class 2 material for high-duty spot and seam welding electrodes, continuous-casting mould components and heat-exchange parts that run hot under load.

Nifty Alloys supplies C18150 / CuCr1Zr chromium zirconium copper from Dubai, UAE, in round bar and plate / block, in the precipitation hardened TH04 condition to EN 12163 and RWMA Class 2. Stock bar and plate are cut to length or block size and dispatched with EN 10204 3.1 Mill Test Certificates as standard, reporting certified, traceable chemistry, hardness and electrical conductivity; EN 10204 3.2 third-party inspection is available on request. We deliver across the UAE within 24–48 hours, to Saudi Arabia, Kuwait, Qatar, Oman and Bahrain within 3–5 working days, and export to Europe, India and Africa for automotive welding lines, electrode manufacturers and fabrication plants. Send your size list or electrode drawing to request a quote — quotations are turned around the same day.

Chemical Composition

Cu

Copper

1 %
Cr

Chromium

0.5 – 1.2 %

0.1 %
Zr

Zirconium

0.03 – 0.3 %

Fe

Iron

≤ 0.08 %

Si

Silicon

≤ 0.1 %

Others

total

≤ 0.2 %

Typical value Range (min–max) Minimum (≥) Maximum (≤) Hover / tap for notes

Standard

EN 12163

EN

Revision: EN 12163 — current edition

Copper and copper alloys - rod for general purposes. European standard covering CuAl10Ni5Fe4 (CW307G) and other copper alloy rod and bar products.

European standard for C63200 / CuAl10Ni5Fe4 wrought rod and bar. CW307G is the EN numeric code for the wrought form. CC333G is the EN casting designation. Also see EN 12167 (profiles) and EN 12168 (hollow sections).

Available Forms

Plate / Block

10–100 mm. Thickness; blocks saw-cut to size. [VERIFY — stock range not confirmed]

Round Bar

10–150 mm. Diameter, precipitation hardened. Hardness minimum falls with size per RWMA Class 2. [VERIFY — stock range not confirmed]

Stock & delivery

Stock location
Dubai, UAE
In stock
Precipitation Hardened (TH04) to EN 12163 / RWMA Class 2 — the only stocked condition. Forms and sizes held in Dubai per current stock list.
Delivery UAE
24–48 hours
Delivery GCC
3–5 working days — Saudi Arabia, Kuwait, Qatar, Oman, Bahrain
Export
Europe, India, Africa on request
Quotation
Same-day quotation
Minimum order
No minimum order quantity for standard sizes

Key standards

EN 12163

Designations & Equivalents

StandardDesignationNotes
UNSC18150Primary designation — Unified Numbering System
DINCuCr1ZrGerman / European chemical designation
EN / Werkstoff2.1293German material number (former DIN 17666)
EN NameCuCr1ZrEN 12163 chemical designation
EN / WerkstoffCW106C(EN Number) EN numerical designation
Common NameEN 12163(EN Standard) Rod for general purposes — primary European standard
Common NameEN 12164 [VERIFY — CuCr1Zr listing in EN 12164 not confirmed](EN Standard) Named in the register; CuCr1Zr is confirmed in EN 12163, EN 12165 and EN 12167
Common NameRWMA Class 2 (Group A)(RWMA) Resistance-welding electrode classification — AWS J1.3
ISOISO 5182 A2/2International electrode material designation
Common NameNo AMS or MIL specification applies(AMS / MIL) No AMS or military specification covers C18150 — supplied to EN 12163 / RWMA Class 2.
ASTMNo ASTM product specificationASTM B441 covers beryllium coppers C17500 / C17510 / C17465 — not C18150.
Common NameCuCrZr / chromium zirconium copper / copper chromium zirconium / chrome zirconium copper / Class 2 copperBuyer search terms

Compliance & Certification

StandardStatusNotes
EN 10204 3.1SuitableProvided as standard — chemistry, hardness and electrical conductivity to EN 12163 / RWMA Class 2.
EN 10204 3.2ConditionalAvailable on request with independent third-party inspection — specify at order stage.

Specifications

Mechanical Properties

Values per EN 12163. Bar length compares conditions within each row.

PropertyPrecipitation Hardened (TH04) | EN 12163
Tensile Strength (UTS)470 MPaminRoom temp — 4 to 25 mm (R470)EN 12163 minimum.
Tensile Strength (UTS)420 MPaminRoom temp — over 25 to 50 mm (R420)EN 12163 minimum.
Yield Strength (0.2% Proof Stress)380 MPatypicalRoom temp — 4 to 25 mmApproximate value given for information in EN 12163 — not a requirement.
Yield Strength (0.2% Proof Stress)330 MPatypicalRoom temp — over 25 to 50 mmApproximate value given for information in EN 12163 — not a requirement.
Elongation8 %minA (5.65√So) — 4 to 25 mmEN 12163 minimum (R470).
Elongation12 %minA (5.65√So) — over 25 to 50 mmEN 12163 minimum (R420).
Hardness75 HRBminTypical 80 HRBUp to 25 mmRWMA Class 2 minimum. Typical 72–83 HRB (125–155 HB) across bar sizes.
Hardness70 HRBminOver 25 to 50 mmRWMA Class 2 minimum.
Hardness65 HRBminOver 50 mmRWMA Class 2 minimum.

Physical Properties

PropertyPrecipitation Hardened (TH04) | EN 12163
Densityat 20°C8.89 g/cm³
Modulus of Elasticityat 20°C117 GPa
Thermal Conductivityat 20°C324 W/m·K
Coefficient of Thermal Expansionat 20–300°C17.1 µm/m·°C
Specific Heat Capacityat 20°C380 J/kg·K
Electrical Conductivityat 20°C80 % IACS
Electrical Resistivityat 20°C0.02 µΩ·m
Melting Point / Rangeat Solidus–Liquidus1070 °C

Service Conditions

Service Temperature

Max 350 °C

Notes

The alloy is stable to about 350–370°C (700°F) under load, and hardened material retains its mechanical properties with good ductility in the 300–500°C range for limited exposures. Above the ageing range the precipitates coarsen and hardness, strength and conductivity fall progressively; zirconium delays this compared with C18200 but does not stop it. Electrode faces see higher temperatures only transiently and are water cooled. As an FCC copper alloy it has no ductile-to-brittle transition; low-temperature use is not restricted.

Corrosion Performance

General corrosion

Good atmospheric and fresh-water corrosion resistance and good oxidation resistance at electrode temperatures. Attacked by ammonia, oxidising acids (nitric) and sulphur-bearing atmospheres at temperature. Keep cooling water clean and deionised where specified to avoid internal scaling and erosion. Sour service: copper alloys are not certified to NACE MR0175 — not applicable to this grade.

Pitting resistance

Behaves like high-conductivity copper: good resistance in fresh and cooling water as used in water-cooled electrodes and mould plates, with low pitting risk in clean circuits. Not designed for seawater immersion — for seawater duty select a nickel aluminium bronze.

Additional notes

Not applicable — PREN applies to stainless steels and nickel alloys.

Heat Treatment

HEAT TREATMENT GUIDE — C18150 / CuCr1Zr / 2.1293

Solution treatment: 982–1010°C — short soak to dissolve chromium and zirconium, avoiding excessive grain growth — rapid water quench — soft, supersaturated solid solution, low conductivity. Cold working: draw or roll after quenching — increases final strength and accelerates ageing (TH04 route). Precipitation hardening (ageing): about 425–500°C — 2–4 h (reference practice about 427°C / 800°F for 3 h) — air cool — fine Cr and Zr-rich precipitates; restores conductivity to about 80% IACS and reaches R470 / RWMA Class 2 properties. Hot working: 816–927°C (1500–1700°F); hot forgeability good. Over-ageing / softening: exposure above the ageing range (brazing, welding, overheating in service) coarsens precipitates and softens the alloy — properties are recovered only by a new solution treatment, quench and age. No heat treatment is needed after machining hardened stock.

ENGINEERING NOTES
Weldability
Fair

C18150 can be joined by gas-shielded arc welding (GTAW / GMAW), soldering and brazing; oxy-fuel welding and resistance welding of the alloy itself are not recommended. Any joining operation that heats the metal above the ageing range over-ages or re-solutionises the precipitates, so the heat-affected zone loses the hardness and conductivity of the hardened temper; only a new solution treatment and age restores them. Zirconium raises the softening threshold compared with C18200 but does not prevent softening at brazing temperatures. Preheat thicker sections when arc welding because of copper's high thermal conductivity, and use a suitable flux when brazing. Where full properties are required, machine the part from hardened bar and keep joints away from working faces.

Filler metals
  • ERCu · AWS A5.7 / TIG (GTAW)Deoxidised copper filler for joining to copper — weld and HAZ will be softer than the hardened parent
  • ERCu · AWS A5.7 / MIG (GMAW)For thicker sections; preheat required because of copper's heat conductivity
  • BAg series · AWS A5.8 / BrazingSilver brazing alloys with flux for electrode shanks and holders; brazing softens the joint zone
Machinability
Fair

Machinability rating 20 (free-cutting brass C36000 = 100). Machine in the precipitation hardened condition as supplied — no heat treatment is needed afterwards. The alloy is tough and produces long, stringy chips: use sharp, polished carbide or HSS tools with high positive rake, chip-breaker geometry, generous coolant and moderate speeds. Avoid rubbing cuts, which work harden the surface and degrade electrode face finish.

Applications

  • Spot welding electrode caps and tips for galvanised and coated automotive body steels
  • Seam welding wheels for coated-steel tanks, drums and HVAC duct fabrication
  • Electrode holders, shanks and adaptors on robotic resistance welding guns
  • Projection welding electrodes and inserts for nut and stud welding cells
  • Continuous-casting mould plates and tube components in steel plants
  • Water-cooled heat-exchange parts and cooling plates under high heat flux
  • Switchgear contacts and current-carrying components that run hot under load
  • Mould inserts and hot runner components needing fast heat extraction
  • Flash and butt welding dies and clamping jaws for GCC steel fabricators
  • Welding fixtures and platens for resistance welding cells in UAE manufacturing

Frequently Asked Questions

Quick answers on our grades, certification, supply and lead times.

Still have questions?

Our team responds fast with specifications, certification and stock availability.

Contact our team

C18150 chromium zirconium copper is used mainly for high-duty resistance welding electrodes — spot welding caps and tips, seam welding wheels, projection electrodes and electrode holders — especially for galvanised and coated steels, where its zirconium addition reduces sticking and extends tip life. It is also used for continuous-casting mould components, water-cooled heat-exchange parts, switchgear contacts and mould inserts that run hot under load. In the UAE and GCC, typical buyers are automotive welding lines, electrode makers and steel fabricators.

Get in touch

Elevateyourprojectswithoursuperiorsteel