Alloy Steel dealers in UAE

EN16 / 605M36 / EN16T Alloy Steel | Supplier in UAE & GCC

EN16 / 605M36 / EN16T — Mn-Mo through-hardening steel, EN16T 850–1000 MPa with excellent ductility and freedom from temper brittleness; shafts, bolts, gears.

Industries Served

Automotive
Heavy Engineering
Oil & Gas
Mining
Manufacturing
Construction

Overview

EN16 (BS 970 605M36, supplied heat treated as EN16T / 605M36T) is a manganese-molybdenum through-hardening alloy steel containing 0.32–0.40% carbon, 1.30–1.70% manganese and 0.22–0.32% molybdenum, with no chromium or nickel. Manganese provides most of the hardenability at low cost, while molybdenum deepens hardening and gives the grade its well-known freedom from temper brittleness. Hardened and tempered to Condition T, EN16T delivers 850–1000 MPa tensile strength, 248–302 HB and good impact toughness, with excellent ductility and shock resistance; Condition R (700–850 MPa) suits larger sections. The grade is readily machinable in the supplied condition and offers an economical alternative to chromium and nickel-chromium high-tensile steels where sections are moderate. There is no current EN equivalent and the nearest US grade, SAE 4037, has lower manganese — quoted equivalences to SAE 4135 or 42CrMo4 are incorrect because those are chromium-molybdenum steels. BS 970 itself is withdrawn, and 605M36 continues as a legacy specification.

Nifty Alloys supplies EN16 / 605M36 / EN16T alloy steel from stock in Dubai, UAE, in round bar and flat bar, hardened and tempered to Condition T as standard, with Condition R, Condition S and annealed material on request. Bars are cut to length and dispatched with EN 10204 3.1 Mill Test Certificates as standard, certifying 605M36 chemistry, condition, tensile, impact and hardness results with full traceability to the mill; EN 10204 3.2 third-party inspection is available on request. We deliver across the UAE within 24–48 hours, to Saudi Arabia, Kuwait, Qatar, Oman and Bahrain within 3–5 working days, and export to Europe, India and Africa. Send your size list or drawing to request a quote — quotations are turned around the same day.

Chemical Composition

0.36 %
C

Carbon

0.32 – 0.4 %

Si

Silicon

0.1 – 0.4 %

1.5 %
Mn

Manganese

1.3 – 1.7 %

0.27 %
Mo

Molybdenum

0.22 – 0.32 %

P

Phosphorus

≤ 0.035 %

S

Sulfur

≤ 0.04 %

Typical value Range (min–max) Minimum (≥) Maximum (≤) Hover / tap for notes

Standard

BS 970-1 (withdrawn)

Other

Revision: BS 970-1:1996 (withdrawn — legacy specification)

Available Forms

Round Bar

10–250 mm. Diameter, Condition T in smaller sections; larger sizes in Condition R / S or as rolled subject to ruling section. [VERIFY — stock range not confirmed]

Flat Bar

10–100 mm. Thickness; width × thickness to order. [VERIFY — stock range not confirmed]

Stock & delivery

Stock location
Dubai, UAE
In stock
H&T Condition T (EN16T) — standard stocked condition. Condition R, Condition S and annealed on request.
Delivery UAE
24–48 hours
Delivery GCC
3–5 working days — Saudi Arabia, Kuwait, Qatar, Oman, Bahrain
Export
Europe, India, Africa on request
Quotation
Same-day quotation
Minimum order
No minimum order quantity for standard sizes

Key standards

BS 970-1 (withdrawn)

Designations & Equivalents

StandardDesignationNotes
BSEN16 / EN16T / EN16ROriginal BS 970:1955 designations; T / R = strength condition
BS605M36 / 605M36TBS 970 designation (withdrawn standard) — governing chemistry
BS606M36Free-machining (higher sulphur) variant — not the standard grade
AISI / SAE4037 — nearest onlySame Mo level but lower Mn (0.70–0.90%) — not an exact equivalent
EN NameNo EN equivalent(EN / DIN) No current EuroNorm Mn-Mo grade matches 605M36. SAE 4135 and 42CrMo4 / 1.7225, sometimes quoted, are Cr-Mo steels and are NOT equivalents.
Common NameEN16T round bar / manganese molybdenum steel / Mn-Mo high tensile steel / 55-ton steelBuyer search terms

Compliance & Certification

StandardStatusNotes
EN 10204 3.1SuitableProvided as standard — 605M36 chemistry, condition, tensile, impact and hardness.
EN 10204 3.2ConditionalAvailable on request with independent third-party inspection — specify at order stage.
NACE MR0175 / ISO 15156Requires ConfirmationLow-alloy steel with < 1% Ni — may be acceptable under ISO 15156-2 at 22 HRC maximum in the Q&T condition with other conditions met. Condition T (248–302 HB) exceeds 22 HRC; Condition R (201–255 HB) may meet it only if hardness is controlled to ≤ 237 HB. Confirm against project requirements and hardness testing.

Specifications

Mechanical Properties

Values per BS 970-1 (withdrawn). Bar length compares conditions within each row.

PropertyH&T Condition T (EN16T) | BS 970-1H&T Condition R | BS 970-1Annealed | BS 970-1
Tensile Strength (UTS)850–1000 MPaCondition TBS 970 605M36 range.700–850 MPaCondition RBS 970 605M36 range.–
Yield Strength (0.2% Proof Stress)680 MPaminCondition TBS 970 605M36 minimum (some sources: 650 MPa).525 MPaminCondition RPublished minimum (some sources: 480 MPa).–
Elongation13 %minA (5.65√So)BS 970 605M36 minimum.17 %minA (5.65√So)Published minimum (some sources: 16%).–
Impact Energy (Charpy V-notch)50 JminRoom temp, KCVPublished Condition T value (some sources: 35 J).28 JminRoom temp, KCVPublished Condition R value.–
Hardness248–302 HBCondition TBS 970 range (about 25–32 HRC).201–255 HBCondition RBS 970 range.–AnnealedMaximum reported on MTC [VERIFY — annealed hardness limit not confirmed].

Physical Properties

PropertyH&T Condition T (EN16T) | BS 970-1H&T Condition R | BS 970-1Annealed | BS 970-1
Densityat 20°C7.85 g/cm³7.85 g/cm³7.85 g/cm³
Modulus of Elasticityat 20°C205 GPa205 GPa205 GPa
Thermal Conductivityat 20°C42 W/m·K42 W/m·K42 W/m·K
Coefficient of Thermal Expansionat 20–100°C12 µm/m·°C12 µm/m·°C12 µm/m·°C

Service Conditions

Service Temperature

Max 350 °C

Notes

[VERIFY — maxServiceTempC 350: continuous load-bearing limit not confirmed in a code source] Do not use at or near the tempering temperature. Molybdenum gives freedom from temper brittleness, but tempering between 250 and 375°C must still be avoided because it seriously reduces impact values. Not a creep-resisting grade; specify impact testing for sub-zero service.

Corrosion Performance

General corrosion

Corrodes like carbon steel. High-tensile fasteners in Condition T are susceptible to hydrogen embrittlement from electroplating — bake after plating.

Pitting resistance

No pitting resistance. Rusts in humid and coastal atmospheres typical of the UAE and GCC; protect with oil, paint, phosphate or zinc coatings.

Additional notes

Not applicable — low-alloy steel.

Heat Treatment

HEAT TREATMENT GUIDE — EN16 / 605M36 / EN16T

Forging: start about 1150–1200°C, finish above about 850°C; cool slowly. Softening: heat slowly to 640–660°C and cool in air for machining [VERIFY — annealed hardness not confirmed]. Hardening: 840–870°C — soak to uniform temperature — quench in oil. Temper as soon as parts reach hand warm. Tempering: select temperature from a tempering chart for the required condition — soak 2 h per 25 mm of ruling section — cool in air. Avoid tempering at 250–375°C (seriously reduces impact values). Conditions: R 700–850 MPa (201–255 HB); S 775–925 MPa (223–277 HB); T 850–1000 MPa (248–302 HB). Higher conditions are limited by ruling section [VERIFY — BS 970 limiting ruling sections for 605M36 not confirmed]. Surface hardening: flame or induction hardening of the Condition T bar for local wear resistance. Stress relieving: below the final tempering temperature after heavy machining or welding.

ENGINEERING NOTES
Weldability
Fair

Weldable with precautions — 0.36% carbon and 1.5% manganese give a carbon equivalent around 0.7, so the HAZ hardens readily. Preheat to about 200–300°C [VERIFY — preheat range not confirmed], use dry low-hydrogen consumables, keep interpass at preheat and cool slowly, then stress relieve below the tempering temperature. Welding EN16T reduces the HAZ to uncontrolled properties; avoid welding highly stressed parts.

Filler metals
  • E8018-D3 · AWS A5.5 / SMAWLow-hydrogen Mn-Mo electrode — matches the alloy system
  • ER80S-D2 · AWS A5.28 / TIG / MIGMn-Mo wire for GTAW / GMAW
  • E7018 · AWS A5.1 / SMAWUnder-matching low-hydrogen electrode for non-critical repairs
Machinability
Good

Readily machinable in Condition T (248–302 HB) — one of the grade's main advantages. Carbide tooling recommended for production work; HSS adequate for general turning. Annealed or Condition R material machines more easily for heavy roughing.

Applications

  • High-tensile bolts, studs and nuts for heavy engineering assemblies
  • Drive shafts, axles and spindles for pumps, gearboxes and conveyors
  • Crankshafts and connecting rods for engines and compressors
  • Gears and pinions in moderate sections
  • High-load couplings and hubs for rotating equipment in GCC plants
  • Lifting gear components, shackle pins and hook shanks
  • Pistons and hydraulic components needing shock resistance
  • Anti-roll bars, suspension pins and steering parts for vehicles
  • Machine-tool spindles and arbors
  • Mining and quarry pins and bushings under shock loads

Frequently Asked Questions

Quick answers on our grades, certification, supply and lead times.

Still have questions?

Our team responds fast with specifications, certification and stock availability.

Contact our team

EN16 / 605M36 is used for high-tensile bolts, studs and nuts, shafts, axles, crankshafts, connecting rods, gears, high-load couplings and lifting-gear components — parts that need more strength and shock resistance than EN8 without the cost of a chromium-nickel steel. Supplied as EN16T it gives 850–1000 MPa tensile strength. In the UAE and GCC it is widely used for fasteners, pump shafts and general heavy-engineering repairs.