Bronze dealers in UAE

UNS C63200 / CDA 632 / CA632 Nickel Aluminium Bronze | Supplier in UAE & GCC

UNS C63200 (CDA 632) — quench-and-temper wrought nickel aluminium bronze: 620 MPa min tensile, superior seawater corrosion resistance, MIL-B-24059 naval grade.

Industries Served

Marine
Aerospace & Defence
Oil & Gas
Petrochemical
Power Generation
Mining
Heavy Engineering

Overview

UNS C63200 (CDA 632, CA632) is a wrought nickel aluminium bronze supplied to ASTM B150 for rod and bar, ASTM B124 for forging stock and ASTM B171 for plate, and to MIL-B-24059 for US Navy and defence procurement. Its composition — 8.7–9.5% aluminium, 4.0–4.8% nickel, 3.5–4.3% iron and 1.2–2.0% manganese, with iron held at or below nickel — is tighter than general-purpose NAB, and that balance is what allows a controlled heat treatment. Rod and bar are water quenched from 850°C minimum and temper annealed at 700 ± 15°C, changing the morphology of the kappa phases and removing the continuous phase networks that cause selective phase corrosion in seawater. In the resulting TQ50 temper this aluminium bronze meets 620 MPa minimum tensile strength, 275–345 MPa minimum 0.5% yield strength depending on section, and 15% minimum elongation, while remaining non-sparking and of low magnetic permeability. The nearest European wrought NAB, CuAl10Ni5Fe4 (CW307G), is a different composition and not an exact equivalent.

Nifty Alloys supplies UNS C63200 nickel aluminium bronze from Dubai, UAE, in round bar, hollow bar, flat bar, hexagonal bar and plate / block, in the TQ50 condition to ASTM B150, with ASTM B124 forging stock, ASTM B171 plate and MIL-B-24059 supply available on request. Stock lengths are cut to size and dispatched with EN 10204 3.1 Mill Test Certificates as standard, giving certified, traceable chemistry and tensile results; EN 10204 3.2 third-party inspection and classification-society witnessing are available on request. We deliver across the UAE within 24–48 hours, to Saudi Arabia, Kuwait, Qatar, Oman and Bahrain within 3–5 working days, and export to Europe, India and Africa for naval, offshore and desalination projects. Send your drawing or size list to request a quote — quotations are turned around the same day.

Chemical Composition

Cu

Copper, incl. Ag

9.1 %
Al

Aluminium

8.7 – 9.5 %

4.4 %
Ni

Nickel, incl. Co

4 – 4.8 %

3.9 %
Fe

Iron

3.5 – 4.3 %

1.6 %
Mn

Manganese

1.2 – 2 %

Si

Silicon

≤ 0.1 %

Pb

Lead

≤ 0.02 %

Typical value Range (min–max) Minimum (≥) Maximum (≤) Hover / tap for notes

Standard

ASTM B150 / B150M

ASTM

Revision: B150 / B150M — current edition

Standard specification for aluminium bronze rod, bar, and shapes. Covers C61300, C61400, C62300, C63000, C63200, and other wrought aluminium bronze alloys.

Primary North American standard for C63200 wrought bar and rod. Specifies chemical composition, mechanical properties, and temper designations. Most widely referenced for aluminium bronze bar in UAE and GCC oil & gas and marine procurement.

Available Forms

Flat Bar

10–100 mm. Thickness; width × thickness cut to order. [VERIFY — stock range not confirmed]

Hexagonal Bar

12–100 mm. Across flats. [VERIFY — stock range not confirmed]

Hollow Bar

40–300 mm. Outside diameter; bore to stock or drawing. [VERIFY — stock range not confirmed]

Plate / Block

10–100 mm. Thickness, ASTM B171 hot rolled; blocks saw-cut to size. [VERIFY — stock range not confirmed]

Round Bar

25–300 mm. Diameter, TQ50 to ASTM B150 (heat treatment mandatory to 300 mm). Larger diameters on request. [VERIFY — stock range not confirmed]

Stock & delivery

Stock location
Dubai, UAE
In stock
TQ50 Quench Hardened & Temper Annealed (ASTM B150) — the only stocked condition. Forms and sizes held in Dubai per current stock list. ASTM B171 hot-rolled plate, ASTM B124 forging stock and MIL-B-24059 supply on request.
Delivery UAE
24–48 hours
Delivery GCC
3–5 working days — Saudi Arabia, Kuwait, Qatar, Oman, Bahrain
Export
Europe, India, Africa on request
Quotation
Same-day quotation
Minimum order
No minimum order quantity for standard sizes

Key standards

ASTM B150 / B150M

Designations & Equivalents

StandardDesignationNotes
UNSC63200Primary designation — Unified Numbering System
Common NameCDA 632(CDA) Copper Development Association alloy number
Common NameCA632 / C632 / Alloy 632Trade shorthand used on drawings and RFQs
ASTMB150 / B150MRod, bar and shapes — TQ50 / TQ55
ASTMB124 / B124MForging rod, bar and shapes
ASTMB171 / B171MPlate — hot rolled
Common NameMIL-B-24059(MIL) Rod, bar, shapes and forgings — quench hardened and temper annealed (US Navy procurement)
Common NameQQ-C-465(Federal (cancelled)) Cancelled federal specification — legacy drawings only; supply now to ASTM B150 / MIL-B-24059
AMSNo AMS appliesNo AMS specification covers wrought C63200. AMS 4880 is a cast aluminium bronze specification and does not apply.
EN NameCuAl10Ni5Fe4 — nearest onlyNearest European wrought NAB (EN 12163 / EN 12165). Different composition — NOT an exact equivalent. Primary grade of the C63000 page.
EN / WerkstoffCW307G — nearest only(EN Number (nearest)) As above — nearest, not equivalent.
Common NameWrought NAB / Navy NAB / nickel aluminium bronze / aluminium nickel bronze / aluminum bronze C63200Buyer search terms — includes US spelling "aluminum"

Compliance & Certification

StandardStatusNotes
EN 10204 3.1SuitableProvided as standard with every supply — chemistry and tensile results to ASTM B150 (bar) or B171 (plate).
EN 10204 3.2ConditionalAvailable on request with independent third-party inspection — specify at order stage.
Classification Society Approval (ABS / DNV / LR)Requires ConfirmationWitnessing or approval for classed marine components arranged on request — confirm society and rule requirements at enquiry.
MIL-B-24059ConditionalSupplied on request for defence and naval procurement — confirm specification revision and supplementary test requirements at enquiry.

Specifications

Mechanical Properties

Values per ASTM B150 / B150M. Bar length compares conditions within each row.

PropertyTQ50 Quench Hardened & Temper Annealed | ASTM B150
Tensile Strength (UTS)620 MPaminTypical 670 MPaRoom temp, longitudinalASTM B150 minimum, all sizes to 300 mm. Typical value marked typical.
Yield Strength (0.5% Extension Under Load)345 MPaminRoom temp — section up to 80 mmASTM B150 minimum. Typical 330–380 MPa across sizes.
Yield Strength (0.5% Extension Under Load)310 MPaminRoom temp — section over 80 to 125 mmASTM B150 minimum.
Yield Strength (0.5% Extension Under Load)275 MPaminRoom temp — section over 125 to 300 mmASTM B150 minimum.
Elongation15 %minTypical 18 %5.65√So gauge (min 25 mm)ASTM B150 minimum. Typical value marked typical.
Hardness200 HBtypicalCross-sectionNot specified in ASTM B150 for C63200 — typical 180–230 HB (92–97 HRB).
Impact Energy (Charpy V-notch)25 JtypicalRoom temp, V-notchTypical 23–27 J — not a B150 requirement.

Physical Properties

PropertyTQ50 Quench Hardened & Temper Annealed | ASTM B150
Densityat 20°C7.64 g/cm³
Modulus of Elasticityat 20°C117 GPa
Shear Modulusat 20°C44 GPa
Poisson's Ratioat 20°C0.34 -
Thermal Conductivityat 20°C35 W/m·K
Coefficient of Thermal Expansionat 20–300°C16.2 µm/m·°C
Specific Heat Capacityat 20°C440 J/kg·K
Electrical Conductivityat 20°C7 % IACS
Electrical Resistivityat 20°C0.25 µΩ·m
Melting Point / Rangeat Solidus–Liquidus1041 °C

Service Conditions

Service Temperature

Max 400 °C

Notes

[VERIFY — maxServiceTempC 400: continuous load-bearing limit for C63200 not confirmed in a producer or code source] Copper-base NAB has no ductile-to-brittle transition of the steel type, so sub-zero marine service is routine; confirm impact requirements against the project specification for cryogenic duty. Strength falls progressively above about 300°C. Keep service well below the 700°C temper anneal temperature — prolonged exposure in the 400–700°C range can coarsen the tempered structure and reduce seawater corrosion resistance.

Corrosion Performance

General corrosion

Excellent in seawater, brackish water, brine and desalination streams; good in many non-oxidising acids and alkalis. Avoid oxidising acids (nitric), ammonia-rich media and sulphide-polluted seawater. Galvanically compatible with other copper alloys; will corrode preferentially when coupled to stainless steel, titanium or nickel alloys of larger area in seawater. Sour service: ISO 15156-3 only cautions on copper alloys and mills do not certify them to NACE — NACE MR0175 is not stated for this grade.

Pitting resistance

Very good resistance to pitting, crevice attack, cavitation and erosion-corrosion in flowing seawater, from a self-healing alumina-rich surface film. The TQ50 quench-and-temper treatment was developed specifically to eliminate selective phase (de-aluminification) attack of the kappa phase that can occur in as-worked or as-cast NAB under stagnant or crevice conditions. Weld HAZs not re-tempered remain the most susceptible zone.

Additional notes

Not applicable — PREN applies to stainless steels and nickel alloys. Seawater performance of copper alloys is judged by phase stability, flow-velocity tolerance and galvanic position.

Heat Treatment

HEAT TREATMENT GUIDE — UNS C63200 / CDA 632 / CA632

Quench hardening: 850°C minimum — hold 1 h minimum at temperature — quench in water (or other suitable medium) — retains high-temperature beta, transformed to a hard martensitic structure. Temper anneal (TQ50): 700 ± 15°C — 3 to 9 h at temperature as required for the target properties — air cool — tempers the martensite to alpha + fine, well-distributed kappa phases; gives TQ50 properties (620 MPa min UTS, 15% min elongation) and maximum resistance to selective phase corrosion in seawater. Section limit: per ASTM B150, the quench-and-temper is not mandatory for sections over 300 mm. Annealing: 621–704°C (1150–1300°F) — air cool — softening and stress relief of worked material. Hot working: 816–899°C (1500–1650°F); hot forgeability good. Post-weld: re-apply the 700 ± 15°C temper anneal (3 h minimum) where weld HAZ corrosion resistance matters. No heat treatment is needed after machining TQ50 stock.

ENGINEERING NOTES
Weldability
Good

C63200 welds well by GTAW (AC or DCEN with argon / argon-helium) and pulsed GMAW (DCEP) using matching nickel aluminium bronze filler; SMAW is used mainly for repair. The tenacious alumina film must be removed by wire brushing and cathodic cleaning. No preheat is normally required; keep interpass temperature at or below 150°C [VERIFY — source not confirmed] to limit time in the range where coarse, corrosion-prone phases form. Welding destroys the tempered TQ50 structure in the HAZ: for seawater-wetted parts where full resistance to selective phase corrosion is required, re-apply the ASTM B150 temper anneal (700 ± 15°C, 3 h minimum, air cool) after welding. Never use nickel-free aluminium bronze filler (ERCuAl-A2) on seawater parts — the weld metal becomes anodic to the parent. Oxy-fuel welding is not recommended.

Filler metals
  • ERCuNiAl · AWS A5.7 / TIG (GTAW)Matching NAB filler — preferred for joining and build-up of C63200
  • ERCuNiAl · AWS A5.7 / MIG (GMAW)Pulsed spray transfer for thicker sections and higher deposition
  • ECuNiAl · AWS A5.6 / SMAWCovered electrode for repair and site welding
  • MIL-CuNiAl · MIL-E-23765/3Military filler designation — specify on US Navy / MIL-B-24059 contracts
Machinability
Fair

Machinability rating 30 (free-cutting brass C36000 = 100). Machine in the TQ50 condition as supplied — no further heat treatment is needed after machining. Use carbide tooling with positive rake and rigid set-ups at moderate speeds; chips are tough and stringy, so use chip-breaker geometry and flood coolant. Avoid tool dwell and light rubbing cuts. Typical hardness 180–230 HB.

Applications

  • Seawater pump shafts, wear rings and impeller hubs for ship and offshore cooling systems
  • Valve stems, bonnets and seats for seawater and firewater valves on GCC offshore platforms
  • Propeller shafts, propeller hub hardware and rudder bushings for naval and patrol craft
  • Seawater intake and brine pump components in Gulf desalination and power plants
  • Studs, bolts, nuts and valve stem nuts for seawater-wetted bronze assemblies
  • Bearing cages, sleeve bearings and heavy-duty bushings under high load and shock
  • Non-sparking hand tools and weapon-handling components for explosive atmospheres
  • Accumulator heads, hydraulic fittings and subsea ROV hardware for work-boat service
  • Low magnetic permeability housings and fittings for naval instrumentation systems
  • Firefighting system components and deluge valve parts for offshore installations
  • Wear plates, slides and gibs for mining and heavy engineering equipment

Frequently Asked Questions

Quick answers on our grades, certification, supply and lead times.

Still have questions?

Our team responds fast with specifications, certification and stock availability.

Contact our team

C63200 is used for seawater-wetted shafting, valve and pump components, propeller hardware, fasteners and heavy-duty bushings in naval, offshore and marine service. Its quench-and-temper TQ50 condition gives 620 MPa minimum tensile strength together with resistance to cavitation, erosion and selective phase corrosion in seawater. It is also chosen for non-sparking tools and weapon-handling equipment, low magnetic permeability instrument fittings, and seawater intake and brine pump parts in UAE and GCC desalination and power plants.