Stainless Steel dealers in UAE

17-4PH / 1.4542 / UNS S17400 Precipitation Hardening Stainless Steel | Supplier in UAE & GCC

17-4PH (1.4542 / UNS S17400) — PH stainless steel aged to 860–1310 MPa tensile, with corrosion resistance close to 304 and a NACE-compliant H1150D option.

Industries Served

Oil & Gas
Aerospace & Defence
Marine
Petrochemical
Power Generation
Food Processing
Manufacturing
Medical

Overview

17-4PH stainless steel (EN 1.4542 / X5CrNiCuNb16-4, UNS S17400, AISI Type 630, JIS SUS630) is a martensitic precipitation-hardening stainless steel containing 15.0–17.5% chromium, 3.0–5.0% nickel, 3.0–5.0% copper and 0.15–0.45% niobium. Solution treatment at 1040 °C produces a low-carbon lath martensite; a single ageing step between 482 °C and 621 °C then precipitates fine copper-rich particles that raise strength without a quench, so distortion is minimal. The ageing temperature sets the property balance: H900 gives a minimum tensile strength of 1310 MPa per ASTM A564, H1025 gives 1070 MPa with markedly better toughness, and the double-aged H1150D condition (860 MPa minimum, 24–33 HRC) meets the 33 HRC limit of NACE MR0175 / ISO 15156-3 for sour service. Corrosion resistance is broadly comparable to 304 in atmospheric and mild chemical media, and useful strength is retained to about 300 °C. Because parts can be machined in Condition A and aged afterwards with only 0.05–0.10% shrinkage, 17-4PH is widely specified for valve stems, pump shafts, aerospace fittings and high-strength fasteners.

Nifty Alloys supplies 17-4PH / 1.4542 from stock in Dubai, UAE, as round bar, together with open-die forgings and seamless rolled ring forgings made to drawing. Material is supplied in Condition A for customers who machine before ageing, and in H900, H1025, H1075 and NACE-compliant H1150D for finished-part production, to ASTM A564, ASTM A705 or EN 10088-3 as the project requires. Every delivery is certified with EN 10204 3.1 Mill Test Certificates confirming chemistry, heat treatment and mechanical properties, with full traceability to the mill heat; EN 10204 3.2 third-party inspection is available on request. We deliver within 24–48 hours across the UAE and in 3–5 working days to Saudi Arabia, Kuwait, Qatar, Oman and Bahrain, with export to Europe, India and Africa on request. Contact our team to request a quote and confirm the right ageing condition for your component.

Chemical Composition

0.04 %
C

Carbon

≤ 0.07 %

0.6 %
Mn

Manganese

≤ 1 %

0.4 %
Si

Silicon

≤ 1 %

P

Phosphorus

≤ 0.04 %

S

Sulfur

≤ 0.03 %

15.5 %
Cr

Chromium

15 – 17.5 %

4.3 %
Ni

Nickel

3 – 5 %

3.3 %
Cu

Copper

3 – 5 %

0.3 %
Nb + Ta

Niobium + Tantalum

0.15 – 0.45 %

Mo

Molybdenum

≤ 0.6 %

Fe

Iron

Typical value Range (min–max) Minimum (≥) Maximum (≤) Hover / tap for notes

Standard

ASTM A564 / A564M

ASTM

Revision: ASTM A564/A564M — current edition [VERIFY — confirm edition year against latest mill MTC]

Standard Specification for Hot-Rolled and Cold-Finished Age-Hardening Stainless Steel Bars and Shapes. Covers 17-4PH (Type 630) in all aging conditions.

Related: ASTM A693 (sheet/plate), ASTM A705 (forgings), ASME SA564 (pressure vessel). All share same chemistry.

Available Forms

Forging / Ring Forging

Open-die forgings (discs, blocks, stepped shafts) made to drawing. Leave min/max blank — sizes confirmed per enquiry [VERIFY — confirm maximum forging weight/dimension with supply partner].

Forging / Ring Forging

Seamless rolled rings to drawing (OD, ID, height). Leave min/max blank — sizes confirmed per enquiry [VERIFY].

Round Bar

10–300 mm. Diameter range as stated on the current niftyalloys.com page [VERIFY — confirm against current Dubai stock list before publishing]. Cut to length. Larger diameters to order.

Stock & delivery

Stock location
Dubai, UAE
In stock
Round bar: H1025 and Condition A [VERIFY — the current page states round bar is stocked primarily in H1150; confirm actual stock conditions]. H900, H1075 and H1150D round bar, and all forgings / ring forgings: supplied to order.
Delivery UAE
24–48 hours
Delivery GCC
3–5 working days — Saudi Arabia, Kuwait, Qatar, Oman, Bahrain
Export
Europe, India, Africa on request
Quotation
Same-day quotation
Minimum order
No minimum order quantity for standard sizes

Key standards

ASTM A564 / A564M

Designations & Equivalents

StandardDesignationNotes
Common Name17-4PHPrimary market designation — also written 17-4 PH, 17/4PH, 17-4
UNSS17400Unified Numbering System
AISI / SAEType 630AISI type number — also written AISI 630, SS 630, Grade 630
EN / Werkstoff1.4542European material number per EN 10088-3
EN NameX5CrNiCuNb16-4EN chemical designation
DINX5CrNiCuNb16-4DIN EN designation (DIN EN 10088-3); legacy DIN name X5CrNiCuNb17-4 [VERIFY — legacy name not confirmed against superseded DIN 17440]
JISSUS630JIS G4303 (bar) / JIS G4304–G4305 (plate, sheet)
ISOX5CrNiCuNb16-4ISO 15510 designation
Common Name05Cr17Ni4Cu4Nb(GB) GB/T 20878 / GB/T 1220 — older name 0Cr17Ni4Cu4Nb [VERIFY]
ASTMA564 / A705 / A693 Type 630Bars and shapes / forgings / plate-sheet-strip
ASMESA564 / SA705 Type 630ASME BPVC Section II equivalents
AMSAMS 5643 / AMS 5622 / AMS 5604Bars & forgings / remelted bars & forgings / sheet-strip-plate
EN / Werkstoff1.4548Aerospace (LN/WL) material number used for 17-4PH aerospace quality — confirm against project specification before treating as interchangeable with 1.4542

Compliance & Certification

StandardStatusNotes
EN 10204 3.1SuitableMill Test Certificate provided as standard with every delivery, all conditions and forms.
EN 10204 3.2ConditionalAvailable on request — specify at order stage. Third-party inspector and additional lead time apply.
NACE MR0175 / ISO 15156ConditionalAcceptable ONLY in the H1150D condition — solution treated, then double aged at 621 °C (4 h + 4 h) — with hardness ≤ 33 HRC. H900, H1025 and H1075 are NOT acceptable. ISO 15156-3 also lists equipment-specific restrictions for UNS S17400 — check the applicable table for the component type [VERIFY — confirm against the edition named in the project specification].
NACE MR0103Requires ConfirmationUNS S17400 is listed for refinery sour service in a double-aged (H1150D / H1150M) condition with a hardness limit [VERIFY — confirm the current MR0103 clause and hardness limit before quoting]. Not acceptable in H900–H1075.
AMS 5643ConditionalSupplied to AMS 5643 on request from aerospace-approved mill sources. Hardness must fall within the AMS ranges, which are tighter than ASTM A564 minimums.
ASME SA564 / SA705Requires ConfirmationFor pressure equipment — confirm required ASME edition, Section VIII allowable-stress basis and any code-case requirements at enquiry stage.

Specifications

Mechanical Properties

Values per ASTM A564 / A564M. Bar length compares conditions within each row.

PropertyH1025 | ASTM A564/A564MCondition A | ASTM A564/A564MH1075 | ASTM A564/A564MH1150D | ASTM A564/A564MH900 | ASTM A564/A564M
Tensile Strength (UTS)1070 MPaminTypical 1170 MPaRoom temp, longitudinalMinimum per ASTM A564 H1025. Typical value from producer data.1100 MPatypicalRoom temp, longitudinalNo requirement in ASTM A564 Condition A. Typical value only [VERIFY — producer data].1000 MPaminTypical 1140 MPaRoom temp, longitudinalMinimum per ASTM A564 H1075. Typical value from producer data.860 MPaminRoom temp, longitudinalMinimum per ASTM A564 H1150D. Typical value not entered [VERIFY — add producer typical if available].1310 MPaminTypical 1380 MPaRoom temp, longitudinalMinimum per ASTM A564 H900. Typical value from producer data.
Yield Strength (0.2% Proof Stress)1000 MPaminTypical 1140 MPaRoom temp, longitudinalMinimum per ASTM A564 H1025. Typical value from producer data.760 MPatypicalRoom temp, longitudinalNo requirement in ASTM A564 Condition A. Typical value only [VERIFY — producer data].860 MPaminTypical 1035 MPaRoom temp, longitudinalMinimum per ASTM A564 H1075. Typical value from producer data.725 MPaminRoom temp, longitudinalMinimum per ASTM A564 H1150D.1170 MPaminTypical 1275 MPaRoom temp, longitudinalMinimum per ASTM A564 H900. Typical value from producer data.
Elongation12 %minTypical 15 %50 mm (4D) gauge lengthMinimum per ASTM A564. Typical value from producer data.10 %typical50 mm (4D) gauge lengthNo requirement. Typical value only.13 %minTypical 16 %50 mm (4D) gauge lengthMinimum per ASTM A564. Typical value from producer data.16 %min50 mm (4D) gauge lengthMinimum per ASTM A564.10 %minTypical 14 %50 mm (4D) gauge lengthMinimum per ASTM A564. Typical value from producer data.
Reduction of Area45 %minTypical 56 %LongitudinalMinimum per ASTM A564. Typical value from producer data.45 %typicalLongitudinalNo requirement. Typical value only.45 %minTypical 58 %LongitudinalMinimum per ASTM A564. Typical value from producer data.50 %minLongitudinalMinimum per ASTM A564.40 %minTypical 50 %LongitudinalMin 40% for sections ≤ 75 mm; min 35% for 75–200 mm per ASTM A564. Typical value from producer data.
Hardness35–42 HRCTypical 38 HRCSurface, Rockwell CASTM A564 specifies 35 HRC / 331 HB MINIMUM (no max). Max 42 HRC (401 HB) is the AMS 5643 range upper limit — applies only when ordered to AMS. Typical value from producer data.38 HRCmaxTypical 33 HRCSurface, Rockwell CMaximum per ASTM A564: 38 HRC / 363 HB. EN 10088-3 +AT: 360 HB max. Typical value from producer data.32 HRCminTypical 36 HRCSurface, Rockwell CASTM A564: 32 HRC / 311 HB MINIMUM. AMS 5643 range 311–375 HB when ordered to AMS. Typical value from producer data.24–33 HRCSurface, Rockwell CSpecified RANGE per ASTM A564: 24–33 HRC / 255–311 HB. 33 HRC max is also the NACE MR0175 / ISO 15156-3 limit.40–47 HRCTypical 44 HRCSurface, Rockwell CASTM A564: 40 HRC / 388 HB MINIMUM. Max 47 HRC is the AMS 5643 range upper limit (388–444 HB). Typical value from producer data.
Impact Energy (Charpy)20 JminTypical 47 JRoom temp, V-notch, longitudinalASTM A564 minimum where impact testing is specified on the order [VERIFY — supplementary requirement wording]. Typical value from producer data.–27 JminTypical 54 JRoom temp, V-notch, longitudinalASTM A564 minimum where impact testing is specified [VERIFY — supplementary requirement wording]. Typical value from producer data.41 JminRoom temp, V-notch, longitudinalASTM A564 minimum where impact testing is specified [VERIFY — supplementary requirement wording].20 JtypicalRoom temp, V-notch, longitudinalNo impact requirement in ASTM A564 for H900 — lowest toughness of all conditions. Typical value only [VERIFY].

Physical Properties

PropertyH1025 | ASTM A564/A564MCondition A | ASTM A564/A564MH1075 | ASTM A564/A564MH1150D | ASTM A564/A564MH900 | ASTM A564/A564M
Densityat 20 °C7.81 g/cm³7.81 g/cm³7.81 g/cm³–7.81 g/cm³
Modulus of Elasticityat 20 °C197 GPa197 GPa197 GPa–197 GPa
Thermal Conductivityat 100 °C18.3 W/m·K18.3 W/m·K18.3 W/m·K–18.3 W/m·K
Coefficient of Thermal Expansionat 20–100 °C10.8 µm/m·°C10.8 µm/m·°C10.8 µm/m·°C–10.8 µm/m·°C
Specific Heat Capacityat 20 °C460 J/kg·K460 J/kg·K460 J/kg·K–460 J/kg·K
Melting Point / Rangeat Solidus–liquidus1404 °C1404 °C1404 °C–1404 °C
ISO 9001:2015at Quality Management System — procurement, stock management and supply of special steel products.–––2026 Check current certificate–
AEO (Authorised Economic Operator)at Customs compliance for secure UAE and GCC trade.––––UAE Federal Customs Authority–
1–––1150 Default SpecSheet is H1025 (confirmed in Round 1). stockInfo flagged [VERIFY] — confirm which conditions are physically in stock. H1150 (single age) is not one of the five selected SpecSheets.–
2–––10 Carried into 7.7a and FAQ 6 with a [VERIFY] flag — not independently confirmable.–
3––––Marine application: "propeller shafts … exposed to saltwater".–
4––––Nuclear industry: "reactor components, waste casks".–
5–––1.45 Incorrect — that designation belongs to 1.4594 (FV520B type). 1.4542 = X5CrNiCuNb16-4. Correct the hub tables on /products/stainless-steel and /products/precipitation-hardening-stainless-steel.–
6––––Meta description begins with the literal text "Meta:".–
7–––1 Replaced per slug-rules.md. 301 redirect required (see Reference File Actions).–
8–––17 ASTM A564 hardness values are MINIMUMS for aged conditions (H1025 35 HRC min). This document uses minimums and gives AMS 5643 upper limits separately. Recommend correcting the sample file.–

Service Conditions

Service Temperature

Max 300 °C

Notes

Maximum continuous service approx. 300 °C. Longer exposure in the 300–480 °C range causes further precipitation and 475 °C-type embrittlement, sharply reducing impact toughness, so the alloy is not used for sustained elevated-temperature service. No minimum is entered because 17-4PH is not intended for cryogenic service: toughness falls with temperature, most severely in H900 and H1025. Overaged conditions (H1075, H1150D) retain better low-temperature toughness — where sub-zero service is specified, require Charpy testing at the design temperature on the order.

Corrosion Performance

PREN 16

General corrosion

Good resistance in rural, urban and mild industrial atmospheres, fresh water, steam, many petroleum products and food environments. Coastal atmospheres in the Gulf produce light surface staining over time. Avoid cathodic-protection overprotection and hydrogen charging on high-strength conditions (H900, H1025) — hydrogen embrittlement risk. Passivation after machining and a fine surface finish improve field performance.

Pitting resistance

Pitting resistance is similar to 304 and well below 316L, duplex 2205 and super duplex. In flowing seawater 17-4PH performs adequately, but in stagnant seawater, under deposits and in crevices (seals, threads, sleeves) pitting and crevice corrosion develop. Stress corrosion cracking resistance improves markedly as ageing temperature increases: H900 is the most susceptible in warm chloride or H2S environments; H1025 and above are preferred, and H1150D is the condition for sour service.

PREN notes

Approximate, from PREN = %Cr + 3.3 %Mo + 16 %N using nominal composition (≈16% Cr, no intentional Mo or N). 17-4PH is selected for strength with moderate corrosion resistance — not for chloride pitting resistance.

Heat Treatment

ProcessTemperatureCoolingResult & notes
HEAT TREATMENT GUIDE17-4PH / 1.4542 / X5CrNiCuNb16-4 (per ASTM A564 / A705; EN 10088-3 equivalents shown) Hot working: Heat to 1150–1180 °C and finish above 1010 °C. Do not forge below 1010 °C. After forging, cool to room temperature and solution treat before ageing [VERIFYconfirm forging window with forge procedure]. Solution treatment (Condition A / EN +AT): 1040 ± 15 °C30 min minimum at temperature (longer for heavy sections) — air cool or oil quench to below 32 °C to complete the martensite transformation (Mf ≈ 30 °C) — 38 HRC / 363 HB max (EN +AT: 360 HB max). H900: Condition A + 482 °C — 1 h — air cool — UTS ≥ 1310 MPa, YS ≥ 1170 MPa, 40 HRC min. H1025 (EN +P1070 ≈ 550 °C / 4 h): Condition A + 552 °C — 4 h — air cool — UTS ≥ 1070 MPa, YS ≥ 1000 MPa, 35 HRC min. H1075: Condition A + 579 °C — 4 h — air cool — UTS ≥ 1000 MPa, YS ≥ 860 MPa, 32 HRC min. H1150D (NACE): Condition A + 621 °C — 4 h — air cool to below 32 °C, then 621 °C — 4 h — air cool — UTS ≥ 860 MPa, YS ≥ 725 MPa, 24–33 HRC. Other ASTM A564 conditions on request: H925 (496 °C/4 h), H1100 (593 °C/4 h, ≈ EN +P960), H1150 (621 °C/4 h, ≈ EN +P930), H1150M (760 °C/2 h + 621 °C/4 h, ≈ EN +P800). Dimensional change: ageing produces a uniform contraction of approx. 0.05% (H900) to 0.10% (H1150 range). Finish-machine in Condition A with allowance, then age. Re-treatment: an aged part can be returned to Condition A by re-solution treating at 1040 °C and then re-aged to a different condition. Material must be fully cooled below 32 °C after solution treatment before ageing — incomplete transformation leaves retained austenite and low aged hardness.
ENGINEERING NOTES
Weldability
Good

Weldable by GTAW, GMAW, SMAW and EBW with matching ER630 / E630 consumables. Weld in Condition A or in an overaged condition (H1150 / H1150D) — never in H900, where residual stress and low ductility raise the cracking risk. Preheat is not normally required; for sections over approx. 25 mm or high-restraint joints, preheat 100–150 °C and keep interpass below 150 °C [VERIFY — confirm against the qualified WPS]. Post-weld: for full properties, re-solution treat at 1040 °C, cool below 32 °C and re-age to the specified condition; where re-solution treatment is impractical, ageing directly after welding is acceptable but weld-metal properties will be lower. For NACE MR0175 / ISO 15156-3 service, welded assemblies must receive the full solution treatment plus H1150D double age and meet 33 HRC max in weld, HAZ and parent metal.

Filler metals
  • ER630 · AWS A5.9 / TIG (GTAW)Matching 17-4PH composition — responds to post-weld ageing. Preferred for root and fill passes.
  • ER630 · AWS A5.9 / MIG (GMAW)Matching composition wire for semi-automatic welding of thicker sections.
  • E630-15 / E630-16 · AWS A5.4 / SMAWMatching covered electrode. Keep electrodes dry (low-hydrogen practice).
  • AMS 5825 · AMS / TIG-MIG wireAerospace-quality matching filler wire for AMS-specified components.
  • ER309L · AWS A5.9 / TIG-MIG (dissimilar)For joining 17-4PH to carbon or austenitic steels where weld metal ageing response is not required. Lower weld-metal strength.
Machinability
Good

Best machined in Condition A (38 HRC / 363 HB max) or in H1150D; H900 is the most demanding condition. Use rigid set-ups and carbide tooling with positive rake and generous coolant — the alloy work-hardens and has low thermal conductivity (approx. 18 W/m·K). Machining in Condition A and ageing afterwards is standard practice: ageing causes a uniform contraction of approx. 0.05% (H900) to 0.10% (H1150 range) — leave allowance on precision dimensions. Ageing forms a light temper oxide that is removed by light grinding or pickling.

Applications

  • Valve stems, gates and seat rings for oil & gas gate and ball valves
  • Downhole tool parts, packer components and completion hardware in H1150D for sour wells
  • Pump and compressor shafts for GCC petrochemical, refinery and desalination plant duty
  • Aerospace fittings, actuator components and high-strength fasteners to AMS 5643
  • High-strength studs, bolts and coupling pins for process plant and topside equipment
  • Gas and steam turbine compressor blades, shafts and fixings operating up to 300 °C
  • Boat propeller shafts and rudder stocks in H1075 or H1150D, with crevice-free seal design
  • Ring-forged seal housings, bearing retainers and flanges for rotating equipment
  • Food processing machinery shafts, cutter blades and wear parts needing stainless hygiene
  • Surgical and orthopaedic instrument components to ASTM F899
  • Plastic mould inserts, jigs and fixtures machined in Condition A then aged

Frequently Asked Questions

Quick answers on our grades, certification, supply and lead times.

Still have questions?

Our team responds fast with specifications, certification and stock availability.

Contact our team

17-4PH is used for components that need high strength together with stainless corrosion resistance — valve stems, pump and compressor shafts, aerospace fittings, high-strength fasteners and downhole oil & gas tools. In the oil & gas sector it is specified in H1150D for sour-service parts, while aerospace buyers order it to AMS 5643 for fittings and actuator parts. It is also used for turbine compressor blades, food machinery shafts, surgical instruments and plastic mould inserts. Across the UAE and GCC, the largest demand comes from valve, pump and petrochemical equipment manufacturers.

Get in touch