Stainless Steel dealers in UAE

15-5PH / 1.4545 / UNS S15500 PH Stainless Steel | Supplier in UAE & GCC

15-5PH / 1.4545 / UNS S15500 — Cr-Ni-Cu precipitation-hardening stainless: up to 1310 MPa UTS (H900), tougher than 17-4PH; aerospace, valves, shafts.

Industries Served

Aerospace & Defence
Oil & Gas
Marine
Power Generation
Food Processing

Overview

15-5PH (UNS S15500, ASTM A564 Type XM-12, AMS 5659, 1.4545 / X5CrNiCu15-5) is a martensitic precipitation-hardening stainless steel containing 14.0–15.5% chromium, 3.5–5.5% nickel, 2.5–4.5% copper and 0.15–0.45% niobium plus tantalum. It was developed from 17-4PH with a balanced composition that is essentially free of delta ferrite, which gives better transverse toughness and ductility, more uniform properties in large sections and better forgeability. Supplied in Condition A (solution treated, 38 HRC max) for machining, it is hardened by a single low-temperature ageing treatment between 480°C and 620°C, with very little distortion: H900 reaches 1310 MPa minimum tensile strength and 40–47 HRC, the standard H1025 condition gives 1069 MPa tensile and 1000 MPa yield, and H1075 and H1150 trade strength for higher toughness and stress corrosion cracking resistance. Corrosion resistance is comparable to 17-4PH and better than the hardenable 400-series martensitic grades. Bar to AMS 5659 is consumable-electrode remelted for aerospace cleanliness. Typical uses are aerospace fittings and actuators, valve stems and gates, pump shafts, fasteners and gears.

Nifty Alloys supplies 15-5PH / UNS S15500 stainless steel from Dubai, UAE, in round bar and forgings, in Condition A or aged to H900, H1025, H1075 or H1150, with AMS 5659 remelted material on request. Every supply carries an EN 10204 3.1 Mill Test Certificate as standard, with chemistry, condition, tensile and hardness results; EN 10204 3.2 third-party inspection is available on request. We deliver across the UAE within 24–48 hours, to Saudi Arabia, Kuwait, Qatar, Oman and Bahrain within 3–5 working days, and export to Europe, India and Africa. Send your size list and condition to request a quote — quotations are turned around the same day.

Chemical Composition

0.04 %
C

Carbon

≤ 0.07 %

0.5 %
Mn

Manganese

≤ 1 %

0.5 %
Si

Silicon

≤ 1 %

P

Phosphorus

≤ 0.03 %

S

Sulfur

≤ 0.015 %

14.8 %
Cr

Chromium

14 – 15.5 %

4.5 %
Ni

Nickel

3.5 – 5.5 %

3.4 %
Cu

Copper

2.5 – 4.5 %

0.3 %
Nb + Ta

Niobium + Tantalum

0.15 – 0.45 %

Mo

Molybdenum

≤ 0.5 %

Typical value Range (min–max) Minimum (≥) Maximum (≤) Hover / tap for notes

Standard

ASTM A564 / A564M

ASTM

Revision: ASTM A564 / A564M — current edition (AMS 5659 values identical for bar)

Standard Specification for Hot-Rolled and Cold-Finished Age-Hardening Stainless Steel Bars and Shapes. Covers 17-4PH (Type 630) in all aging conditions.

Related: ASTM A693 (sheet/plate), ASTM A705 (forgings), ASME SA564 (pressure vessel). All share same chemistry.

Available Forms

Forging

100–800 mm. Forged discs, rings and blocks to order. [VERIFY — supply range not confirmed]

Round Bar

10–300 mm. Diameter; Condition A or aged. AMS 5659 properties for bar up to about 300 mm. [VERIFY — stock range not confirmed]

Stock & delivery

Stock location
Dubai, UAE
In stock
Condition A and H1025 [VERIFY — stocked conditions]; H900, H1075, H1150 and double H1150 (H1150D) on request; AMS 5659 remelted on request.
Delivery UAE
24–48 hours
Delivery GCC
3–5 working days — Saudi Arabia, Kuwait, Qatar, Oman, Bahrain
Export
Europe, India, Africa on request
Quotation
Same-day quotation
Minimum order
No minimum order quantity for standard sizes

Key standards

ASTM A564 / A564M

Designations & Equivalents

StandardDesignationNotes
UNSS15500Unified Numbering System
ASTMType XM-12ASTM A564 / A693 / A705 designation
AMSAMS 5659Bar, forgings, rings — remelted (Module 2)
AMSAMS 5862Sheet, strip and plate — aliases only (plate not a stocked form)
AMSAMS 582615-5PH welding wire — aliases only
ASTMA693Plate, sheet and strip — aliases only
EN / Werkstoff1.4545X5CrNiCu15-5 [VERIFY — EN 10088-3 listing not confirmed; may be aerospace EN series only]
EN NameX5CrNiCu15-5European steel name
Common NameZ7CNU15-05(AFNOR) French designation
Common Name15-5PH / 15-5 PH / PH 15-5 / 15Cr-5Ni / XM-12 stainlessBuyer search terms

Compliance & Certification

StandardStatusNotes
EN 10204 3.1SuitableProvided as standard — chemistry, condition, tensile and hardness.
EN 10204 3.2ConditionalAvailable on request with independent third-party inspection — specify at order stage.
NACE MR0175 / ISO 15156Requires ConfirmationISO 15156-3 accepts UNS S15500 only in the double-aged H1150D condition at 33 HRC max [VERIFY — current ISO 15156-3 table]. The listed conditions (A, H900, H1025, H1075, H1150) are not NACE-acceptable as supplied; H1150D available on request.
AMS 5659ConditionalSupplied to AMS 5659 (remelted, aerospace quality) on request — confirm type and revision.

Specifications

Mechanical Properties

Values per ASTM A564 / A564M. Bar length compares conditions within each row.

PropertyH1025 | ASTM A564Condition A | ASTM A564H1075 | ASTM A564H1150 | ASTM A564H900 | ASTM A564
Tensile Strength (UTS)1069 MPaminLongitudinal, bar ≤ 300 mmASTM A564 XM-12 / AMS 5659 minimum.1100 MPatypicalCondition ATypical — not specified.1000 MPaminLongitudinal, bar ≤ 300 mmASTM A564 XM-12 / AMS 5659 minimum.931 MPaminLongitudinal, bar ≤ 300 mmASTM A564 XM-12 / AMS 5659 minimum.1310 MPaminLongitudinal, bar ≤ 300 mmASTM A564 XM-12 / AMS 5659 minimum.
Yield Strength (0.2% Proof Stress)1000 MPaminLongitudinalSpecified minimum.–862 MPaminLongitudinalSpecified minimum.724 MPaminLongitudinalSpecified minimum.1172 MPaminLongitudinalSpecified minimum.
Elongation12 %min4D gauge, longitudinalSpecified minimum.–13 %min4D gauge, longitudinalSpecified minimum.16 %min4D gauge, longitudinalSpecified minimum.10 %min4D gauge, longitudinalSpecified minimum.
Reduction of Area45 %minLongitudinalSpecified minimum.–45 %minLongitudinalSpecified minimum.50 %minLongitudinalSpecified minimum.35 %minLongitudinalSpecified minimum.
Hardness331–401 HBBrinellSpecified range.363 HBmaxCondition ASpecified maximum.311–375 HBBrinellSpecified range.277–352 HBBrinellSpecified range.388–444 HBBrinellSpecified range.
Hardness35–42 HRCRockwell CSpecified range.38 HRCmaxCondition ASpecified maximum.32–39 HRCRockwell CSpecified range.28–37 HRCRockwell CSpecified range.40–47 HRCRockwell CSpecified range.

Physical Properties

PropertyH1025 | ASTM A564Condition A | ASTM A564H1075 | ASTM A564H1150 | ASTM A564H900 | ASTM A564
Densityat 20°C7.8 g/cm³7.8 g/cm³7.8 g/cm³7.8 g/cm³7.8 g/cm³
Modulus of Elasticityat 20°C196 GPa196 GPa196 GPa196 GPa196 GPa
Shear Modulusat 20°C77 GPa77 GPa77 GPa77 GPa77 GPa
Thermal Conductivityat 100°C17.8 W/m·K17.8 W/m·K17.8 W/m·K17.8 W/m·K17.8 W/m·K
Coefficient of Thermal Expansionat 20–93°C11.9 µm/m·°C11.9 µm/m·°C11.9 µm/m·°C11.9 µm/m·°C11.9 µm/m·°C
Electrical Resistivityat 20°C0.77 µΩ·m0.77 µΩ·m0.77 µΩ·m0.77 µΩ·m0.77 µΩ·m

Service Conditions

Service Temperature

Max 316 °C

Notes

Retains strength and corrosion resistance to about 316°C (600°F). Prolonged exposure near or above the ageing temperature overages and reduces strength; long exposure at about 300–400°C can reduce toughness. Low-temperature toughness is best in H1075 / H1150; specify impact testing for sub-zero service.

Corrosion Performance

General corrosion

Better general corrosion resistance than 410 / 420 / 431 martensitic grades. Resistance to stress corrosion cracking increases with ageing temperature — H900 is most susceptible; H1025 and above are preferred for chloride or SCC-prone service.

Pitting resistance

Moderate pitting resistance — adequate for atmospheric and mild chloride service; not for stagnant seawater immersion without protection.

Additional notes

Not normally quoted for PH grades (no Mo / N); corrosion resistance comparable to 17-4PH and to 304 in many environments.

Heat Treatment

HEAT TREATMENT GUIDE — 15-5PH / 1.4545 / UNS S15500

Solution treatment (Condition A): 1040 ± 15°C, cool to below 32°C (air or oil) — 38 HRC max. Ageing (from Condition A, air cool): H900 480°C 1 h; H925 495°C 4 h; H1025 550°C 4 h; H1075 580°C 4 h; H1100 595°C 4 h; H1150 620°C 4 h; H1150D double 620°C 4 h + 620°C 4 h (NACE); H1150M 760°C 2 h + 620°C 4 h (maximum toughness / machinability). Dimensional change: slight contraction on ageing (about 0.05% H1150 to 0.1% H900 [VERIFY]) — allow when finish machining in Condition A. Re-solution treat before re-ageing if a different condition is required. Weld in Condition A, then re-solution treat and age.

ENGINEERING NOTES
Weldability
Good

Readily welded by GTAW, GMAW, SMAW and other common processes; no preheat normally required. Weld in Condition A (or overaged H1150), then re-solution treat and age for full properties, or age directly after welding where full joint strength is not required. Matching 15-5PH filler (AMS 5826) gives age-hardenable welds; austenitic fillers can be used for non-hardened joints.

Filler metals
  • 15-5PH wire · AMS 5826 / TIG (GTAW)Matching, age-hardenable filler
  • ER630 · AWS A5.9 / TIG / MIG17-4PH-type matching filler — commonly used for 15-5PH
  • E630-16 · AWS A5.4 / SMAWMatching covered electrode
  • ER308L / ER309L · AWS A5.9 / TIG / MIGAustenitic filler for non-hardened joints or dissimilar welds
Machinability
Fair

Machinability in Condition A about 50% of B1112 free-machining steel; machining is often easier in H1150. Because ageing causes only small, predictable dimensional change (slight contraction), parts can be finish-machined in Condition A and then aged.

Applications

  • Aerospace structural fittings, actuator components and landing-gear parts (AMS 5659)
  • Valve stems, gates, seats and trim for oil and gas service
  • Pump shafts, impellers and marine propulsion shafting
  • High-strength fasteners, bolts and pins
  • Gears, cams and couplings needing corrosion resistance
  • Marine gas-turbine compressor components
  • Nuclear and power-generation components
  • Paper-mill and chemical-process equipment
  • Food-processing machinery parts
  • Precision machined parts aged after machining with minimal distortion

Related grades in Stainless Steel

Frequently Asked Questions

Quick answers on our grades, certification, supply and lead times.

Still have questions?

Our team responds fast with specifications, certification and stock availability.

Contact our team

15-5PH is used for parts that need high strength with good toughness and corrosion resistance: aerospace fittings and actuators, valve stems and gates, pump and propeller shafts, high-strength fasteners, gears, marine gas-turbine components and nuclear and paper-mill equipment. In the UAE and GCC it is specified for oil and gas valves and pumps, marine shafting and aerospace MRO work.