Alloy Steel dealers in UAE

AISI 4145 / 4145H Mod Alloy Steel | Supplier in UAE & GCC

AISI 4145 / 4145H Mod — Cr-Mo drill collar steel, Q&T to 285–341 HB and 758 MPa min yield per API Spec 7-1; collars, subs, kellys and stabilisers.

Industries Served

Oil & Gas
Heavy Engineering
Manufacturing
Mining

Overview

AISI 4145 (UNS G41450, with the hardenability-band variant 4145H, UNS H41450, and the mill-modified 4145H Mod) is a chromium-molybdenum alloy steel with 0.43–0.48% carbon, 0.80–1.10% chromium and 0.15–0.25% molybdenum, defined by ASTM A29 and supplied quenched and tempered to meet API Spec 7-1 for rotary drill stem elements. Its higher carbon than 4140 raises attainable hardness, while chromium and molybdenum give the hardenability needed to through-harden large drill-collar sections; 4145H Mod tightens phosphorus and sulphur and raises manganese, chromium or molybdenum within the H-band so that collars up to 11 in OD harden uniformly to the core. Quenched and tempered to 285–341 HB, 4145H Mod meets API Spec 7-1 minimums of 758 MPa yield and 965 MPa tensile for collars up to 6-7/8 in OD, with 54 J average Charpy toughness at room temperature. There is no exact European equivalent — 42CrMo4 has lower carbon and 50CrMo4 higher. 4145 is the standard material for drill collars, subs, kellys, stabiliser bodies and heavy oilfield tools.

Nifty Alloys supplies AISI 4145 / 4145H Mod alloy steel from stock in Dubai, UAE, in round bar, hollow bar and forgings, quenched and tempered to 285–341 HB for API Spec 7-1 drill-collar duty as standard, with annealed bar on request. Bars are ultrasonically tested, cut to length and dispatched with EN 10204 3.1 Mill Test Certificates as standard, reporting chemistry, tensile, Charpy impact and hardness results with full traceability to the mill; EN 10204 3.2 third-party inspection is available on request. We deliver across the UAE within 24–48 hours, to Saudi Arabia, Kuwait, Qatar, Oman and Bahrain within 3–5 working days, and export to Europe, India and Africa for drilling contractors, tool shops and service companies. Send your OD, length and API requirements to request a quote — quotations are turned around the same day.

Chemical Composition

0.45 %
C

Carbon

0.43 – 0.48 %

Mn

Manganese

0.75 – 1 %

Si

Silicon

0.15 – 0.35 %

0.95 %
Cr

Chromium

0.8 – 1.1 %

0.2 %
Mo

Molybdenum

0.15 – 0.25 %

P

Phosphorus

≤ 0.035 %

S

Sulfur

≤ 0.04 %

Ni

Nickel

≤ 0.25 %

Typical value Range (min–max) Minimum (≥) Maximum (≤) Hover / tap for notes

Standard

API Spec 7-1

Other

Revision: API Spec 7-1 — current edition

Specification for Rotary Drill Stem Elements. Covers drill collars, drill pipe, heavy weight drill pipe (HWDP), tool joints, and bottom hole assembly (BHA) components. Defines material grades, mechanical property classes, and testing requirements for 4145H steel.

Published by API (American Petroleum Institute). Primary oil & gas industry standard for drill collar and BHA component procurement. Class 1: min 120 ksi YS / 140 ksi UTS. Class 2: min 135 ksi YS / 150 ksi UTS. Specifies 4145H chemistry, hardenability, and mechanical testing requirements. Mandatory reference for all UAE and GCC drill collar and BHA component supply. Also see API Spec 5D (drill pipe) and API Spec 7-2 (threading).

Available Forms

Forging

200–600 mm. Forged bars and blocks to order. [VERIFY — stock range not confirmed]

Hollow Bar

79–280 mm. Outside diameter; bore to drill-collar size or drawing. [VERIFY — stock range not confirmed]

Round Bar

79–280 mm. Diameter, Q&T 285–341 HB — matches API 7-1 drill-collar range 3-1/8 to 11 in. Smaller diameters on request. [VERIFY — stock range not confirmed]

Stock & delivery

Stock location
Dubai, UAE
In stock
Quenched & Tempered 4145H Mod, 285–341 HB (API Spec 7-1 drill-collar properties) — standard stocked condition. Annealed on request.
Delivery UAE
24–48 hours
Delivery GCC
3–5 working days — Saudi Arabia, Kuwait, Qatar, Oman, Bahrain
Export
Europe, India, Africa on request
Quotation
Same-day quotation
Minimum order
No minimum order quantity for standard sizes

Key standards

API Spec 7-1

Designations & Equivalents

StandardDesignationNotes
AISI / SAE4145Primary designation — ASTM A29 chemistry
UNSG41450Unified Numbering System (4145)
AISI / SAE4145HHardenability-band grade — ASTM A304 / SAE J1268
UNSH41450UNS for 4145H
Common Name4145H Mod / 4145 ModifiedMill designation for drill-collar steel with tightened chemistry — not a standard grade
Common NameAPI Spec 7-1(API) Drill collar / drill stem element mechanical requirements
ASTMA29 / A29MChemistry standard
DIN42CrMo4 / 1.7225 — nearest onlyLower carbon (0.38–0.45% C) — not an equivalent
DIN50CrMo4 / 1.7228 — nearest onlyHigher carbon (0.46–0.54% C), matches AISI 4150 — not an equivalent
JISSCM445Nearest Japanese grade
Common NameDrill collar steel / 4145 round bar / 4145H Mod Q&T / chrome-moly drill collar materialBuyer search terms

Compliance & Certification

StandardStatusNotes
EN 10204 3.1SuitableProvided as standard — chemistry, tensile, Charpy and hardness to API Spec 7-1 / ASTM A29.
EN 10204 3.2ConditionalAvailable on request with independent third-party inspection — specify at order stage.
NACE MR0175 / ISO 15156Not Applicable — Q&T 4145H Mod at 285–341 HB (about 30–37 HRC) exceeds the 22 HRC maximum for carbon and low-alloy steels in ISO 15156-2. Not suitable as supplied for sour service; sour drilling requires a project-specific material selection.
NACE MR0103Not Applicable — Hardness exceeds refinery sour-service limits as supplied.

Specifications

Mechanical Properties

Values per API Spec 7-1. Bar length compares conditions within each row.

PropertyQ&T 285–341 HB | API Spec 7-1Annealed | ASTM A29
Tensile Strength (UTS)965 MPaminOD 79.4 to 174.6 mm (3-1/8 to 6-7/8 in)API Spec 7-1 minimum (140 ksi).–
Tensile Strength (UTS)931 MPaminOD 177.8 to 279.4 mm (7 to 11 in)API Spec 7-1 minimum (135 ksi).–
Yield Strength (0.2% Proof Stress)758 MPaminOD 79.4 to 174.6 mmAPI Spec 7-1 minimum (110 ksi).–
Yield Strength (0.2% Proof Stress)689 MPaminOD 177.8 to 279.4 mmAPI Spec 7-1 minimum (100 ksi).–
Elongation13 %minAll ODsAPI Spec 7-1 minimum.–
Hardness285–341 HB25 mm below surfaceAPI Spec 7-1 range (about 30–37 HRC).200 HBtypicalAnnealed at about 820°C, furnace cooledTypical — not a specification requirement.
Impact Energy (Charpy V-notch)54 JminRoom temp, 25 mm below surface — averageAPI Spec 7-1 average (40 ft-lb); 47 J minimum individual.–

Physical Properties

PropertyQ&T 285–341 HB | API Spec 7-1Annealed | ASTM A29
Densityat 20°C7.85 g/cm³7.85 g/cm³
Modulus of Elasticityat 20°C205 GPa205 GPa
Thermal Conductivityat 20°C42.6 W/m·K42.6 W/m·K
Coefficient of Thermal Expansionat 20–100°C12.3 µm/m·°C12.3 µm/m·°C

Service Conditions

Service Temperature

Max 400 °C

Notes

[VERIFY — maxServiceTempC 400: continuous load-bearing limit not confirmed in a code source] Do not use near or above the tempering temperature, which would reduce hardness below the API 7-1 range; avoid prolonged service in the 350–550°C temper-embrittlement range. Room-temperature Charpy is the API requirement — specify a sub-zero impact test on the order for cold-climate or arctic drilling.

Corrosion Performance

General corrosion

Corrosion-fatigue in mud and brine is a primary drill-collar failure mode — control mud chemistry and inspect connections. Susceptible to sulphide stress cracking at its 285–341 HB hardness in H2S environments; for directional work near magnetic surveys, use non-magnetic stainless collars instead.

Pitting resistance

No pitting resistance. Exposed to drilling mud, brine and humid Gulf atmospheres it corrodes; protect stored collars with rust preventive and thread compounds, and phosphate or coat connections.

Additional notes

Not applicable — low-alloy steel.

Heat Treatment

HEAT TREATMENT GUIDE — AISI 4145 / 4145H Mod / UNS G41450

Forging: start about 1150–1200°C, finish above about 850°C; cool slowly. Normalising: 870–900°C — air cool — refines grain before hardening. Annealing: about 820°C — furnace cool — roughly 200 HB for machining. Hardening: 845–870°C — soak through the full section — quench in oil or polymer. Tempering: temper immediately to 285–341 HB through the full length (API Spec 7-1); tempering temperature set by section and mill practice, typically in the 540–650°C range [VERIFY — exact range not confirmed]. Verification: API Spec 7-1 requires hardness and Charpy testing 25 mm below the surface, and uniform properties along the length. Stress relieving: below the final tempering temperature after heavy machining or welding. Post-machining: cold roll thread roots and stress-relief features on connections.

ENGINEERING NOTES
Weldability
Poor

Not recommended for welding in the Q&T condition — 0.45% carbon with chromium and molybdenum gives a high carbon equivalent and a hard, crack-prone heat-affected zone. Drill-collar hardbanding and repairs need a qualified procedure: preheat to about 260–370°C [VERIFY — preheat range not confirmed], maintain interpass, use dry low-hydrogen consumables, slow cool and post-weld stress relieve below the tempering temperature. Welding across a stress-relief groove or near connections is not permitted on API drill-stem elements.

Filler metals
  • E10018-M · AWS A5.5 / SMAWLow-hydrogen high-strength electrode; preheat and PWHT required
  • ER100S-1 · AWS A5.28 / TIG / MIGHigh-strength wire for near-matching repair welds
  • E8018-B2 · AWS A5.5 / SMAWUnder-matching Cr-Mo electrode where lower joint strength is acceptable
Machinability
Fair

Q&T material at 285–341 HB machines well with carbide tooling, rigid set-ups and flood coolant — threading API connections and trepanning bores are routine in this condition. Annealed material (about 200 HB) machines more easily for heavy roughing before heat treatment. Cold-roll thread roots after machining to improve connection fatigue life.

Applications

  • Slick and spiral drill collars to API Spec 7-1 for GCC onshore and offshore rigs
  • Crossover subs, bit subs, saver subs and lift subs for drill strings
  • Kellys, kelly saver subs and kelly valves for rotary drilling
  • Integral blade and replaceable sleeve stabiliser bodies
  • Drilling jars, shock subs and downhole motor housings
  • Heavy-weight drill pipe tool joints and centre upsets
  • Fishing tools, overshots and reamers for well intervention
  • Mining drill rods, adaptors and blast-hole drilling components
  • Heavy-duty shafts and couplings needing high hardness through large sections
  • Hydraulic cylinder rods and press components under high load

Frequently Asked Questions

Quick answers on our grades, certification, supply and lead times.

Still have questions?

Our team responds fast with specifications, certification and stock availability.

Contact our team

AISI 4145 / 4145H Mod is used mainly for oilfield drill-stem elements — drill collars, subs, kellys, stabiliser bodies, jars and heavy-weight drill pipe tool joints — because it can be through-hardened to 285–341 HB in sections up to 11 in OD. It is also used for mining drill rods and heavy-duty shafts. In the UAE and GCC, drilling contractors, tool shops and service companies buy 4145H Mod Q&T bar to API Spec 7-1 for collar and sub manufacture and repair.