C17200 / CuBe2 / CW101C

C17200 / CuBe2 (2.1247, CW101C) - the highest-strength commercially available copper alloy. UTS up to 1400 MPa HT condition. Available per AMS 4534, AMS 4533, and MIL-C-21657 for aerospace and defence applications. Note: beryllium-containing alloy - observe all applicable health and safety regulations.

Industries Served

Aerospace & Defense
Oil & Gas
Electronics
Manufacturing
Automotive
Medical
Power Generation

Overview

C17200 (EN CuBe2, DIN 2.1247, EN CW101C) is a copper-beryllium alloy containing 1.80-2.00% beryllium and 0.20-0.60% cobalt/nickel in a copper matrix. It is the highest-strength commercially available copper alloy, achieving tensile strengths of 1170-1400 MPa in the HT (precipitation hardened) condition - comparable to alloy steel - while maintaining electrical conductivity of 20-25% IACS and thermal conductivity far exceeding steel. The strength mechanism is analogous to other precipitation-hardening alloys: beryllium dissolves in the copper matrix during solution annealing (AT temper), then precipitates as coherent metastable particles during aging at 315-345 degrees C (HT temper), producing a dramatic increase in hardness and strength. C17200 is specified in aerospace, defence, oil & gas, and electronics applications wherever the unique combination of near-steel strength, copper-class conductivity, non-magnetic properties, non-sparking characteristics, and corrosion resistance is required. Available per AMS 4534, AMS 4533, and MIL-C-21657 for defence and aerospace procurement.

Nifty Alloys supplies C17200 / CuBe2 from stock in Dubai, UAE, in round bar, flat bar/strip, and plate/block in both the HT (precipitation hardened) and AT (solution annealed) conditions. All material is supplied with EN 10204 3.1 Mill Test Certificates as standard - confirming chemical composition, mechanical properties, and hardness. IMPORTANT: C17200 is a beryllium-containing alloy. All machining, grinding, and processing must be conducted in compliance with applicable occupational health and safety regulations (COSHH, UAE Federal Law No. 8, OSHA 29 CFR 1910.1024 as applicable). Nifty Alloys provides material safety data sheets (MSDS/SDS) upon request. We deliver across the UAE within 24-48 hours and export to Saudi Arabia, Kuwait, Qatar, Oman, and Bahrain.

Chemical Composition

Cu

Copper

1.9 %
Be

Beryllium

1.8 – 2 %

0.35 %
Co+Ni

Cobalt plus Nickel

0.2 – 0.6 %

Fe

Iron

≤ 0.15 %

Si

Silicon

≤ 0.2 %

Pb

Lead

≤ 0.02 %

Other

total

≤ 0.5 %

Typical value Range (min–max) Minimum (≥) Maximum (≤) Hover / tap for notes

Standard

ASTM B197 - current edition

Available Forms

Round Bar

Diameter 3-150 mm. Extruded and drawn. Per ASTM B196 / AMS 4534 / MIL-C-21657. For precision pins, shafts, bushings, and electrical contact components. Maximum diameter smaller than steel or copper chromium grades due to beryllium processing constraints. HT (precipitation hardened) standard stock; AT (solution annealed) on request.

Flat Bar

Thickness 3-25 mm, width up to 300 mm. Per ASTM B197 / MIL-C-21657. For springs, contacts, and precision flat components in thicker sections. (Thin gauge below 3 mm is supplied as Strip.) HT and AT conditions.

Strip

Thickness 0.10-3 mm, width up to 300 mm. Per AMS 4533 / MIL-C-21657. For springs, contacts, switch elements, and precision thin-gauge flat components. HT and AT conditions.

Plate

Thickness 6-100 mm. Per ASTM B197. For mould inserts, precision tooling, and large contact components. Cut-to-size available. Smaller maximum thickness than steel due to beryllium alloy production constraints.

Block

Per ASTM B197. For mould inserts and precision tooling blocks. Cut-to-size available on indent.

Designations & Equivalents

StandardDesignationNotes
UNSC17200UNS number
EN NameCuBe2EN / DIN chemical name
EN / WerkstoffCW101CEN material code (CEN designation)
EN / Werkstoff2.1247Werkstoff-Nr. (DIN)
ASTMB197 Alloy C17200ASTM strip/plate specification
ASTMB196 Alloy C17200ASTM rod/bar specification
AMSAMS 4534C17200 rod and bar - aerospace / defence procurement reference
AMSAMS 4533C17200 strip and sheet - aerospace procurement reference
AMSMIL-C-21657C17200 rod, bar, strip, and plate - US DoD military / defence procurement reference (no MIL system in enum; mapped to AMS as the closest procurement-spec system)
ISOISO 1337 CuBe2ISO designation
Common NameBeryllium CopperCommon name
Common NameBeryllium Bronze / BeCuCommon name (variant)

Compliance & Certification

StandardStatusNotes
EN 10204 3.1SuitableEN 10204 3.1 Mill Test Certificate standard with all supply - confirms chemical composition (including Be and Co+Ni content) and mechanical properties.
EN 10204 3.2ConditionalEN 10204 3.2 independent third-party inspection available on request.
AMS 4534ConditionalAerospace rod/bar specification for C17200, available from qualified mill sources - specify clearly at enquiry stage.
AMS 4533ConditionalAerospace strip/sheet specification for C17200, available from qualified mill sources - specify clearly at enquiry stage.
MIL-C-21657ConditionalUS defence procurement specification for C17200 all wrought forms, available from qualified mill sources - specify clearly at enquiry stage. MSDS/SDS available on request for all beryllium copper supply.

Specifications

Mechanical Properties

Bar length compares conditions within each row.

PropertyPrecipitation Hardened HTASTM B197Solution Annealed ATASTM B197
Tensile Strength (UTS)1170–1400 MPaTypical 1275 MPaRoom temp, longitudinalPer ASTM B197 HT. Highest commercial copper alloy. Exact value depends on prior cold work (AT+HT vs H+HT).480–690 MPaTypical 585 MPaRoom temp, longitudinalAT condition per ASTM B197. Wide range depending on exact temper and prior processing.
Yield Strength (0.2% Proof Stress)1000–1200 MPaTypical 1100 MPaRoom temp0.2% offset.170–380 MPaTypical 270 MPaRoom tempLow yield - maximum formability.
Elongation3 %minTypical 5 %50 mm gauge lengthLow elongation in maximum strength condition.20 %minTypical 35 %50 mm gauge lengthExcellent formability for deep drawing and complex forming.
Hardness36–42 HRCTypical 39 HRCRockwell CHT hardness range. Approximately 352-400 HB equivalent.60–80 HRBTypical 70 HRBRockwell BSoft condition. Much lower than HT condition.
Electrical Conductivity20–25 % IACSTypical 22 % IACS20 degrees CMuch lower than C18200/C18150. Acceptable for spring and contact applications. Higher conductivity grades (C17510) available if conductivity is critical.15–22 % IACSTypical 18 % IACS20 degrees CLower than HT due to Be in solid solution. Recovers to 20-25% IACS after aging to HT.
Fatigue Strength500 MPamax10^8 cycles, R=-1Outstanding fatigue life - critical for spring applications. [VERIFY]170 MPamax10^8 cycles, R=-1AT condition - lower than HT. Age to HT before final application. [VERIFY]

Physical Properties

PropertyPrecipitation Hardened HTASTM B197Solution Annealed ATASTM B197
Densityat 20 degrees C8.26 g/cm38.26 g/cm3
Modulus of Elasticityat 25 degrees C131 GPa131 GPa
Thermal Conductivityat 20 degrees C115 W/m.K115 W/m.K
Coefficient of Thermal Expansionat 20-100 degrees C17.8 um/m.degC17.8 um/m.degC
Specific Heat Capacityat 20 degrees C420 J/kg.K420 J/kg.K
Melting Point / Rangeat Solidus865 degrees C865 degrees C

Service Conditions

Service Temperature

Min -200 °CMax 200 °C

Notes

C17200 HT maintains its excellent mechanical properties and fatigue life down to cryogenic temperatures (-200 degrees C) - austenitic behaviour of the copper matrix ensures no brittle transition. Maximum continuous service temperature in HT condition is approximately 150-200 degrees C - above this, over-ageing occurs progressively and strength reduces. For sustained elevated-temperature service above 150 degrees C, consider higher-temperature copper alloys or refractory metals. C17200 is widely used in cryogenic and subsea applications where no lower temperature limit applies in practical service.

Corrosion Performance

General corrosion

Excellent for a high-strength alloy. C17200 has good corrosion resistance in most atmospheric, marine, and chemical environments - comparable to pure copper and significantly better than most steels of equivalent strength. The beryllium addition enhances corrosion resistance vs pure copper. Suitable for seawater, non-oxidising acids, alkalis, and most industrial atmospheres.

Pitting resistance

Good. Better than austenitic stainless steel in some chloride environments due to absence of SCC susceptibility. Not as good as high-alloy stainless or nickel alloys in the most aggressive media.

Additional notes

PREN is not applicable to copper-beryllium alloys (PREN is a stainless-steel pitting index). Crevice corrosion resistance: Good - better than austenitic stainless in seawater. SCC resistance: Very good - C17200 is not susceptible to chloride-induced SCC (unlike austenitic stainless steels), a key advantage for subsea, offshore, and chemical processing applications where high-strength stainless steel components would be at SCC risk. NACE: C17200 is not typically specified under NACE MR0175 for general sour service, but its non-susceptibility to SSC and SCC makes it suitable for downhole tool applications in H2S environments where hardness and strength requirements must be met. Verify specific application against NACE standards at order stage.

Heat Treatment

Note: C17200 precipitation hardening (aging) must be carried out in an inert atmosphere furnace (nitrogen or vacuum). Beryllium surface oxidation occurs in air above approximately 400 degrees C. All heat treatment of C17200 should be outsourced to specialist beryllium-certified heat treatment facilities. Do not age in standard air furnaces.

Solution Annealing (AT temper) - 760-800 degrees C - Water quench (rapid) Resulting condition: AT - 60-80 HRB, conductivity 15-22% IACS, UTS 480-690 MPa. Dissolves Be into solid solution. Water quench mandatory. Perform in inert atmosphere (N2 or vacuum) to prevent surface beryllium oxide formation. Complete all forming, deep drawing, and rough machining in this soft condition.

Cold Work (H temper - optional) - Room temperature - Cold work (no quench) Resulting condition: H - intermediate strength. Optional: cold working after AT and before aging produces the HT series (half-hard + aged). Nifty Alloys HT stock is pre-aged by mill. H+HT (worked then aged) gives higher strength than AT+HT.

Precipitation Hardening (aging to HT) - 315-345 degrees C (optimum 325-335) - Air cool from aging temperature Resulting condition: HT - 36-42 HRC, conductivity 20-25% IACS, UTS 1170-1400 MPa. 2-3 hours. MUST be performed in inert atmosphere (N2 or vacuum) furnace - beryllium oxidises in air above 400 degrees C. Do not use standard air furnaces. Specialist beryllium heat treatment facility required. Verify final hardness and conductivity - confirm HRC and IACS on test certificate.

Over-aging check - Above 345 degrees C Softening begins. Over-aging above 345 degrees C progressively reduces strength and hardness. Unlike C18200/C18150, C17200 has a narrow aging window - temperature control within +/-5 degrees C is important for reproducible properties.

Stress Relief (HT condition) - 150-175 degrees C - Air cool Minimal property change. Low-temperature stress relief to reduce residual machining stress in HT condition. Below the aging temperature so no over-aging occurs. Hold 1-2 hours.

ENGINEERING NOTES
Weldability
Not_recommended

WELDING AND FLAME CUTTING ARE STRONGLY CONTRAINDICATED for C17200. Beryllium oxide fumes generated above 650 degrees C are highly toxic and carcinogenic. If fusion welding is unavoidable in exceptional circumstances: use only in a fully enclosed, purpose-designed beryllium welding facility with LEV extraction and HEPA filtration; respiratory protection (airline supplied-air respirator) mandatory; specialist health and safety assessment required before any welding operation. In almost all applications, silver brazing (BAg-7 or equivalent at 620-680 degrees C in a fume-controlled environment) is the preferred joining method - brazing produces significantly less beryllium oxide fume than fusion welding. Never flame cut C17200 without specialist beryllium extraction equipment. Filler/joining options: AWS BAg-7 silver braze (preferred, fume-controlled environment), AWS BAg-24 silver braze (alternative for less critical joints), and ERCuBe TIG filler (specialist beryllium welding facility only, airline-supplied respirator mandatory).

Machinability
Fair

BERYLLIUM HEALTH AND SAFETY - MANDATORY READING BEFORE MACHINING OR WELDING: Beryllium fumes and dust are highly toxic. Beryllium oxide particles generated during machining, grinding, and especially welding or flame cutting can cause chronic beryllium disease (CBD) - an irreversible, debilitating lung disease - and are classified as a Group 1 human carcinogen (IARC). Engineering controls (wet machining, local exhaust ventilation with HEPA filtration), personal protective equipment (P3/N100 respirator, nitrile gloves, eye protection), and compliance with occupational exposure limits (OEL: 0.00002 mg/m3 chronic, 0.00005 mg/m3 acute - ACGIH TLV) are mandatory. All personnel must be trained in beryllium hazards before handling. Maintain MSDS/SDS on-site at all times. C17200 has good machinability in the AT (solution annealed) condition - approximately 20-30% of free-machining brass machinability index, similar to austenitic stainless steel. All machining MUST be conducted wet (flood coolant mandatory) to prevent beryllium dust generation. NEVER dry machine, dry grind, or dry polish C17200. Use water-based or synthetic coolant (not oil mist). Local exhaust ventilation with HEPA filtration is required. In the HT (hardened) condition, machinability is reduced significantly due to hardness of 36-42 HRC - carbide tooling essential. Preferred sequence: rough machine in AT condition, age to HT, then finish grind or EDM to final dimensions.

Applications

  • Precision springs, snap-action switches, and contact elements in aerospace and defence electronics requiring fatigue resistance and high conductivity
  • Non-sparking tools and safety equipment for use in explosive, flammable, and volatile atmospheres in oil & gas refineries and chemical plants in UAE
  • Downhole oil & gas tools requiring high strength, non-magnetic properties, and corrosion resistance in MWD/LWD (measurement while drilling) instruments
  • Aerospace fasteners, bushings, and structural connectors requiring high strength-to-weight ratio and corrosion resistance per AMS 4534
  • Precision mould components for plastic injection moulding where exceptional thermal conductivity and high hardness must be combined
  • Electrical contact components in high-cycle switching equipment, relay springs, and connector housings requiring fatigue life and conductivity
  • Medical device components including surgical instrument springs, dental handpiece components, and implantable device connectors
  • Underwater connectors, subsea sensor housings, and ROV components requiring non-magnetic, high-strength, and corrosion-resistant properties
  • High-performance gyroscope and inertial navigation system components requiring non-magnetic copper alloy with near-steel strength
  • Resistance welding electrode faces for special applications requiring high hardness and conductivity where C18200/C18150 strength is insufficient

Related grades in Copper Alloys

Frequently Asked Questions

Quick answers on our grades, certification, supply and lead times.

Still have questions?

Our team responds fast with specifications, certification and stock availability.

Contact our team

C17200 (CuBe2, CW101C, 2.1247) is the highest-strength commercially available copper alloy, specified wherever near-steel strength, high conductivity, and non-sparking or non-magnetic properties must be combined. Key applications in UAE and globally include: non-sparking tools and safety equipment for explosive and flammable atmospheres in oil & gas and chemical facilities; precision springs, snap-action switches, and electrical contacts in aerospace and defence electronics; downhole oil & gas MWD/LWD instrument components requiring high strength and non-magnetic properties; aerospace fasteners and structural connectors per AMS 4534; precision mould inserts requiring high hardness and thermal conductivity; subsea connectors and sensor housings for offshore oil & gas; medical device springs and dental handpiece components; and resistance welding electrode faces for special high-hardness applications. Its unique combination of properties makes it irreplaceable in applications where no other material satisfies all requirements simultaneously.