Overview

A2 tool steel (AISI A2 / DIN 1.2363 / X100CrMoV5, UNS T30102) is an air-hardening cold work tool steel containing about 1.0% carbon, 5% chromium, 1% molybdenum and 0.25% vanadium, specified to ASTM A681 and EN ISO 4957. Molybdenum gives it deep hardenability in still air, so tools harden with very little distortion or size change and a low risk of quench cracking. Because it holds about half the chromium of the 12% Cr D-types, A2 forms far fewer primary carbides. It therefore has clearly better toughness and chipping resistance than D2 / 1.2379, with moderate wear resistance between O1 and D2. A2 is hardened from 930–980 °C to 60–63 HRC. It can be tempered low (150–200 °C, about 62 HRC) or high (500–550 °C, about 59 HRC) where nitriding, PVD or wire EDM follow. It is supplied soft annealed to a maximum of 241 HB (EN ISO 4957) / 248 HB (ASTM A681), for blanking, trimming and forming dies, punches, gauges and mould inserts.

Nifty Alloys supplies A2 / 1.2363 / X100CrMoV5 tool steel through our Dubai, UAE facility in round bar, flat bar and plate / block, soft annealed and ready for machining and heat treatment. A2 is supplied on request against your order, while D2 / 1.2379 and O1 / 1.2510 are held in Dubai stock for urgent cold work tooling. Every order carries an EN 10204 3.1 Mill Test Certificate as standard, confirming chemistry and annealed hardness with full traceability to the producing mill. EN 10204 3.2 third-party inspection is available on request. We deliver across the UAE and the GCC — Saudi Arabia, Kuwait, Qatar, Oman and Bahrain — and export to Europe, India and Africa. As an ISO 9001:2015 certified tool steel supplier in the UAE, our team can help you weigh A2 against D2 or S1 for dies that chip or crack in service. Contact our team to request a quote.

Chemical Composition

1 %
C

Carbon

0.95 – 1.05 %

0.3 %
Si

Silicon

0.1 – 0.4 %

0.6 %
Mn

Manganese

0.4 – 0.8 %

P

Phosphorus

≤ 0.03 %

S

Sulfur

≤ 0.03 %

5.2 %
Cr

Chromium

4.8 – 5.5 %

1.1 %
Mo

Molybdenum

0.9 – 1.2 %

0.25 %
V

Vanadium

0.15 – 0.35 %

Ni + Cu
Typical value Range (min–max) Minimum (≥) Maximum (≤) Hover / tap for notes

Standard

EN ISO 4957

EN

Revision: EN ISO 4957:2018 / ASTM A681-08 (2022)

Tool steels — specification for chemical composition, heat treatment, and properties of tool steels including cold work, hot work, and high-speed grades.

Published as BS EN ISO 4957; leading BS dropped to match house style. European standard governing 1.2379 (X153CrMoV12) and other DIN tool steel grades. Supersedes former DIN 17350 for tool steels. Referenced in European and Middle Eastern engineering procurement. Equivalent German standard: DIN EN ISO 4957.

Available Forms

Flat Bar

10–50 mm. Thickness. Widths to order; saw-cut from block where needed. Supplied on request.

Plate / Block

10–300 mm. Thickness. Saw-cut to customer dimensions. Supplied on request.

Round Bar

10–300 mm. Diameter. Typical mill range, supplied on request — confirm size and lead time at enquiry.

Stock & delivery

Stock location
Dubai, UAE
In stock
Annealed — A2 / 1.2363 is supplied on request (not held as Dubai stock); lead time confirmed at quotation. D2 / 1.2379 and O1 / 1.2510 annealed are held in Dubai stock as alternatives. UAE / GCC delivery times apply from dispatch.
Delivery UAE
24–48 hours
Delivery GCC
3–5 working days — Saudi Arabia, Kuwait, Qatar, Oman, Bahrain
Export
Europe, India, Africa on request
Quotation
Same-day quotation
Minimum order
No minimum order quantity for standard sizes

Key standards

EN ISO 4957

Designations & Equivalents

StandardDesignationNotes
AISI / SAEA2Primary designation
UNST30102Unified Numbering System
EN / Werkstoff1.2363European material number. Not to be confused with 1.2365 (X32CrMoV3-3, a hot work steel)
DINX100CrMoV5German designation (formerly X100CrMoV5-1 in DIN 17350)
EN NameX100CrMoV5EN ISO 4957 steel name
ISOX100CrMoV5ISO 4957 designation
ASTMA681 (A2)ASTM product standard
BSBA2BS 4659 — withdrawn, legacy UK designation
JISSKD12Nearest Japanese equivalent (JIS G4404) [VERIFY — source not confirmed]
Common NameZ100CDV5(AFNOR) French designation (legacy)
Common Name95Kh5GM (95Х5ГМ)(GOST) Russian designation
AMSNoneNo AMS specification applies to A2 / 1.2363 — not an aerospace procurement grade
Common NameA2 tool steel, 5% chromium air-hardening tool steel, X100CrMoV5-1Buyer search terms used in UAE / GCC and Europe

Compliance & Certification

StandardStatusNotes
EN 10204 3.1SuitableMill Test Certificate provided as standard. Confirms chemistry and annealed hardness to EN ISO 4957 / ASTM A681.
EN 10204 3.2ConditionalAvailable on request — specify at order stage. Additional lead time and cost may apply.
NACE MR0175 / ISO 15156Not Applicable — A2 is a cold work tool steel used at 57–63 HRC, far above NACE hardness limits. Not used for sour-service pressure-containing parts.

Specifications

Mechanical Properties

Values per EN ISO 4957. Bar length compares conditions within each row.

PropertyAnnealed | EN ISO 4957 / ASTM A681
Hardness (annealed)241 HBmaxSurface, as suppliedMax per EN ISO 4957. ASTM A681 max 248 HB (262 HB cold drawn).
Tensile Strength (UTS)–Room tempNot specified by EN ISO 4957 or ASTM A681 for annealed tool steel — leave blank.
Yield Strength (0.2% Proof Stress)–Room tempNot specified — leave blank.
Elongation–Not specified — leave blank.
Hardness (hardening response)60 HRCminTypical 62 HRC941–954 °C / air / 204 °C temper 2 hMinimum per ASTM A681 Table 3. Typical 62 HRC after 200 °C temper (producer data) — typical.
Hardness (high temper)59 HRCtypicalHardened + 500 °C temperTypical — producer data. Basis for nitriding / EDM practice.

Physical Properties

PropertyAnnealed | EN ISO 4957 / ASTM A681
Densityat 20°C7.7 g/cm³
Modulus of Elasticityat 20°C–[VERIFY — source not confirmed]. Leave blank until confirmed.
Thermal Conductivityat 20°C15.8 W/m·K
Coefficient of Thermal Expansionat 20–100°C11.6 µm/m·°C
Specific Heat Capacityat 20°C–[VERIFY — source not confirmed]. Leave blank until confirmed.
Melting Point / Rangeat Solidus–[VERIFY — source not confirmed]. Leave blank until confirmed.

Service Conditions

Service Temperature

Max 200 °C

Notes

A2 is a cold work steel. The tool must work below its final tempering temperature or it will soften. At the usual 150–200 °C temper (about 62 HRC) the working limit is about 200 °C. Tools tempered at 500–550 °C (about 59 HRC) are more stable against frictional heating, but A2 is not a hot work steel. Hardness falls to about 52 HRC after a 600 °C temper. Use H13 / 1.2344 class steels for hot tooling.

Corrosion Performance

General corrosion

A2 will rust readily in humid or coastal UAE and GCC conditions. Store under cover with rust-preventive oil and protect finished tools between production runs. For corrosion-resistant mould work specify 1.2083 / X40Cr14. Nitriding or PVD coating of high-tempered A2 adds surface wear resistance but does not make it corrosion resistant.

Pitting resistance

No pitting resistance in chloride environments.

Additional notes

Not applicable — tool steel with about 5% Cr. Not corrosion resistant.

Heat Treatment

ProcessTemperatureCoolingResult & notes
HEAT TREATMENT GUIDEA2 / 1.2363 / X100CrMoV5: Soft Annealing: 800–840 °Chold until uniformly heated throughcontrolled slow furnace cooling — max 241 HB (EN ISO 4957) / 248 HB (ASTM A681). Stress Relieving: 600–650 °C — after heavy rough machining or for complex shapes — slow furnace cooling. Carry out before finish machining and hardening. Preheating: In stages at approximately 400 °C, 650 °C and 850 °C (ASTM A681 test preheat: 788 °C). Hardening: Austenitise at 930–980 °C — hold 15–30 min after through-heating — cool in still air, pressurised gas (vacuum furnace) or a 500–550 °C hot bath. Large sections may be oil quenched. Use the gentlest medium that fully hardens the section to minimise distortion. Stop cooling at about 80 °C. Tempering: Temper immediately from about 80 °C. Double temper, 1 hour per 20 mm thickness, minimum 2 hours each. Typical hardness after tempering: 100 °C — 63 HRC; 200 °C — 62 HRC; 300 °C — 59 HRC; 400 °C — 57 HRC; 500 °C — 59 HRC; 600 °C — 52 HRC. Low temper (150–200 °C) for maximum hardness. High temper (500–550 °C) for best stress relief before nitriding, PVD or wire EDM — note the hardness recovery around 500 °C. Hardening response (ASTM A681 test): preheat 788 °C, austenitise 941 °C (salt bath) or 954 °C (controlled atmosphere) for 5–15 min, air cool, single 2 h temper at 204 °C — minimum 60 HRC. Surface Treatment: Nitriding and PVD are suitable on tools tempered at or above the treatment temperature. Post-weld Stress Relief (annealed material): 600–650 °C — furnace cooling.
ENGINEERING NOTES
Weldability
Poor

A2 / 1.2363 is not used for welded joints. At about 1% carbon and air hardening, the weld and heat-affected zone harden on cooling and crack easily. Die repair is possible with preheat, interpass held at or above preheat, low-hydrogen practice and slow cooling under cover [VERIFY — preheat temperature range to be confirmed from producer welding data]. Annealed material should be stress relieved at 600–650 °C after welding; hardened tools must be re-tempered at or just below their original tempering temperature. Ask us before repairing a hardened A2 tool.

Filler metals
  • ER312 · AWS A5.9 / TIG (GTAW)Buffer (buttering) layer on crack-sensitive high-carbon base metal before hard build-up. Not a matching-hardness deposit.
  • Air-hardening cold work matching rod, 54–60 HRC deposit · Tool-steel repair rod / TIG (GTAW)For edge and surface build-up on A2 dies. [VERIFY — consumable code and classification to be confirmed with consumable supplier]
Machinability
Fair

Machine in the soft-annealed condition (≤241 HB). With far fewer primary carbides than D2 or D3, A2 is noticeably easier on cutting tools than the 12% Cr grades. Use coated carbide for milling and turning, and HSS-Co for drilling and tapping. Stress relieve at about 650 °C after heavy rough machining and before finish machining. When tempered at 500–550 °C, hardened A2 can be wire-EDM cut with lower cracking risk. Grind with soft, open wheels and plenty of coolant.

Applications

  • Blanking and piercing dies for medium-gauge sheet where D2 edges chip
  • Trimming dies and punches for automotive body and chassis pressings
  • Bending, forming and coining dies that take repeated shock loading
  • Press-brake punches and bending tools for UAE and GCC fabrication shops
  • Shear blades for medium-thickness plate in steel service centres
  • Master gauges, thread gauges and fixtures needing long-term dimensional stability
  • Injection mould inserts and cores for glass-filled polymers in packaging plants
  • Mandrels, arbors, knurling rolls and embossing rolls
  • Wear parts and guide bushes nitrided or PVD-coated after high-temperature tempering
  • Complex-section punches and die inserts finished by wire EDM after hardening

Frequently Asked Questions

Quick answers on our grades, certification, supply and lead times.

Still have questions?

Our team responds fast with specifications, certification and stock availability.

Contact our team

A2 tool steel (1.2363 / X100CrMoV5) is used for cold work tools that need a balance of toughness, wear resistance and dimensional stability. Typical parts are blanking, piercing and trimming dies, forming and coining dies, press-brake punches, shear blades, gauges, mandrels and mould inserts. Hardened to 60–63 HRC, it resists chipping better than D2 while still wearing well. In the UAE and GCC it is widely used in automotive pressing, fabrication shops and packaging mould makers who need tools that hold size after heat treatment.