Tool Steel dealers in UAE

D2 / 1.2379 / X153CrMoV12 Cold Work Tool Steel | Supplier in UAE & GCC

D2 (1.2379 / X153CrMoV12) — air-hardening 12% chromium cold work tool steel offering high wear resistance, 58–62 HRC working hardness and low distortion.

Industries Served

Automotive
Manufacturing
Mould & Die
Heavy Engineering

Overview

D2 cold work tool steel (AISI D2, UNS T30402, Werkstoff 1.2379, EN ISO 4957 X153CrMoV12, JIS SKD11) is a high-carbon, high-chromium ledeburitic tool steel specified for long-run tooling where abrasive and adhesive wear govern tool life. Its 1.45–1.60% carbon and 11–13% chromium form a large volume of hard M7C3 chromium carbides, while 0.70–1.00% molybdenum and 0.70–1.00% vanadium add hardenability, wear-resistant MC carbides and a secondary hardening response when tempered at 500–550 °C. The grade is supplied soft annealed to a maximum of 255 HB for machining, then hardened from 1000–1080 °C to a working hardness of 58–62 HRC. Because D2 hardens in still air, vacuum or pressurised gas, distortion and size change are low compared with oil-hardening tool steels — the main reason toolmakers select it for precision blanking dies, punches, thread rolling dies and industrial knives.

Nifty Alloys supplies D2 / 1.2379 cold work tool steel from stock in Dubai, UAE, in the soft annealed condition as round bar, flat bar and plate/block, with forgings available for larger or custom sections. Material is certified to ASTM A681 and EN ISO 4957, and every delivery carries an EN 10204 3.1 mill test certificate confirming chemical analysis, annealed hardness and full heat traceability; EN 10204 3.2 third-party inspection is available on request. As an ISO 9001:2015 certified stockist, we deliver within the UAE in 24–48 hours, to Saudi Arabia, Kuwait, Qatar, Oman and Bahrain in 3–5 working days, and to Europe, India and Africa on request. Send us your sizes and quantities to request a quote — our team responds the same day.

Chemical Composition

1.55 %
C

Carbon

1.45 – 1.6 %

0.3 %
Si

Silicon

0.1 – 0.6 %

0.35 %
Mn

Manganese

0.2 – 0.6 %

P

Phosphorus

≤ 0.03 %

S

Sulfur

≤ 0.03 %

12 %
Cr

Chromium

11 – 13 %

0.8 %
Mo

Molybdenum

0.7 – 1 %

0.8 %
V

Vanadium

0.7 – 1 %

Typical value Range (min–max) Minimum (≥) Maximum (≤) Hover / tap for notes

Standard

EN ISO 4957

EN

Revision: EN ISO 4957 — current edition (2018)

Tool steels — specification for chemical composition, heat treatment, and properties of tool steels including cold work, hot work, and high-speed grades.

Published as BS EN ISO 4957; leading BS dropped to match house style. European standard governing 1.2379 (X153CrMoV12) and other DIN tool steel grades. Supersedes former DIN 17350 for tool steels. Referenced in European and Middle Eastern engineering procurement. Equivalent German standard: DIN EN ISO 4957.

Available Forms

Flat Bar

Custom widths and thicknesses — saw-cut from plate/block to order. Sizes on request.

Forging

Open-die forged blocks, discs and rings — size by enquiry with drawing.

Plate / Block

10–400 mm. Thickness range. Width and length cut to order. [VERIFY — confirm against stock list]

Round Bar

10–500 mm. Diameter. Black, peeled or turned. Larger diameters as forged bar on request. [VERIFY — confirm against stock list]

Stock & delivery

Stock location
Dubai, UAE
In stock
Soft annealed (≤255 HB) — round bar, flat bar, plate/block. Forgings on request.
Delivery UAE
24–48 hours
Delivery GCC
3–5 working days — Saudi Arabia, Kuwait, Qatar, Oman, Bahrain
Export
Europe, India, Africa on request
Quotation
Same-day quotation
Minimum order
No minimum order quantity for standard sizes

Key standards

EN ISO 4957

Designations & Equivalents

StandardDesignationNotes
AISI / SAED2Primary designation. Classified under SAE J437 / J438.
UNST30402Unified Numbering System
EN / Werkstoff1.2379European material number
EN NameX153CrMoV12Current EN ISO 4957 chemical designation — primary European name used on this page
DINX155CrVMo12-1Former DIN 17350 designation (withdrawn) — still common on legacy drawings and German mill certificates
ISOX153CrMoV12ISO 4957 designation
BSBD2Former BS 4659 designation (withdrawn — superseded by BS EN ISO 4957)
JISSKD11JIS G4404 near-equivalent — V range 0.20–0.50% differs from 1.2379; not dual-certifiable
ASTMA681 (D2)ASTM alloy tool steel specification
Common NameZ160CDV12Former French AFNOR designation
Common NameCr12Mo1V1Chinese GB/T 1299 equivalent
Common NameD2 tool steel / 12% Cr cold work steelIndustry shorthand used by toolmakers and buyers

Compliance & Certification

StandardStatusNotes
EN 10204 3.1SuitableMill Test Certificate provided as standard — chemical analysis and annealed hardness to ASTM A681 / EN ISO 4957, with heat number traceability.
EN 10204 3.2ConditionalAvailable on request — third-party inspection to be specified at order stage; adds lead time.
SEP 1921Requires ConfirmationUltrasonic testing of bars and blocks — acceptance class to be agreed at enquiry stage. Recommended for large die blocks.
NACE MR0175 / ISO 15156Not Applicable — D2 is a tool steel and is not used for pressure-containing sour-service parts. Hardened D2 (58–62 HRC) far exceeds the 22 HRC general limit for carbon and low-alloy steels.
NACE MR0103Not Applicable — Not applicable — tool steel, not refinery sour-service equipment material.

Specifications

Mechanical Properties

Values per EN ISO 4957. Bar length compares conditions within each row.

PropertyAnnealed | EN ISO 4957
Hardness (annealed)255 HBmaxAs supplied, soft annealedSpecified max — ASTM A681, EN ISO 4957 (+A), JIS G4404. Typically ≤235 HB (typical).
Tensile Strength (UTS)860 MPamaxConverted from 255 HBApproximate maximum by hardness conversion (ISO 18265). Not a specified requirement.
Yield Strength (0.2% Proof Stress)420 MPatypicalRoom temp, annealedNot specified by any standard. Producer-reported approximate value (typical). [VERIFY — source not confirmed]
Elongation–Not specified — annealed tool steel is not tensile-tested in standard supply. [VERIFY — no reliable typical value confirmed]
Hardness — EN ISO 4957 hardening test61 HRCmin1020 ±10 °C, air quench, temper 180 ±10 °CSpecified minimum — confirms the annealed bar responds correctly to hardening. Not an as-supplied value.
Hardness — as quenched63–65 HRCHardened 1020–1040 °CTypical producer data (typical). Reference only.
Hardness — working (hardened & tempered)58–62 HRCTypical 60 HRCAfter hardening + double temperTypical working range (typical). Achieved by customer heat treatment.

Physical Properties

PropertyAnnealed | EN ISO 4957
Densityat 20 °C7.7 g/cm³
Modulus of Elasticityat 20 °C210 GPa
Thermal Conductivityat 20 °C16.7 W/m·K
Coefficient of Thermal Expansionat 20–100 °C10.5 µm/m·°C
Specific Heat Capacityat 20 °C460 J/kg·K
Melting Point / Rangeat Solidus–[VERIFY — solidus not confirmed from a reliable source. Leave blank until confirmed; do not publish an estimated value.]

Service Conditions

Service Temperature

Max 400 °C

Notes

D2 is a cold work tool steel: service temperature is limited by its tempering temperature, not by oxidation. Tools tempered low (150–250 °C) for maximum hardness must stay below their tempering temperature in service — typically under about 150–200 °C — or they will soften. Tools hardened from 1040–1080 °C and tempered at 500–550 °C (secondary hardening route) hold about 58 HRC and can tolerate working temperatures up to about 400 °C. Above roughly 500 °C hardness falls rapidly (about 50 HRC after tempering at 600 °C). No minimum temperature is rated: toughness is low at any temperature, so D2 is not used for impact-loaded or sub-zero structural service. For hot tooling use a hot work steel such as H13 / 1.2344. Guidance value — confirm against the actual tool tempering record.

Corrosion Performance

General corrosion

Better resistance to light staining than low-alloy tool steels, particularly when hardened with a low tempering temperature and polished. Tempering in the 500–550 °C range precipitates further chromium carbides and slightly reduces this resistance. Not stainless — in GCC humidity keep tools oiled and stored dry; specify PVD coating, nitriding or a stainless tool steel (e.g. 1.2083) where corrosion matters.

Pitting resistance

No reliable pitting resistance in chloride environments. Will pit and rust in humid coastal air and in contact with seawater, coolants or process water if left unprotected.

Additional notes

Not applicable — tool steel. PREN does not apply because most of the ~12% chromium is tied up in M7C3 carbides rather than dissolved in the matrix.

Heat Treatment

ProcessTemperatureCoolingResult & notes
HEAT TREATMENT GUIDED2 / 1.2379 / X153CrMoV12: Forging: 1050–850 °C. Do not forge below 850 °C. Cool slowly in the furnace or insulating medium, then soft anneal. Soft annealing: 800–850 °C2–5 hfurnace cool at 10–20 °C/h to about 600 °C, then air — max 255 HB (typically ≤235 HB). Stress relieving: 600–650 °C — 1–2 h after through-heating — slow furnace cool to about 500 °C, then air. Carry out after rough machining and before final machining to minimise hardening distortion. Preheating for hardening: two-stage, approx. 600–650 °C and 850 °C, to equalise temperature in thick sections. Hardening: Route A (maximum hardness, low temper) 1000–1040 °C. Route B (secondary hardening — for nitriding, PVD coating or wire EDM) 1040–1080 °C. Soak about 30 min after the core reaches temperature. Quench in still air, pressurised nitrogen (vacuum furnace), oil, or hot bath 500–550 °C. As-quenched hardness 63–65 HRC. Sub-zero treatment (optional): −70 to −80 °C directly after quenching, before tempering, to transform retained austenite and improve dimensional stability of gauges and precision tools. Tempering: Temper immediately when the tool reaches 50–70 °C. Minimum two tempers, at least 2 h each (about 1 h per 20 mm section), cooling to room temperature between tempers. Typical hardness after hardening from 1020 °C: 200 °C → 61 HRC · 300 °C → 58 HRC · 400–500 °C → 58 HRC · 525 °C → 60 HRC (secondary peak) · 550 °C → 56 HRC · 600 °C → 50 HRC. Nitriding / PVD: Only on tools hardened by Route B and tempered at or above 500 °C; process temperature must stay below the last tempering temperature. Standard hardening test (EN ISO 4957): 1020 ±10 °C, air quench, temper 180 ±10 °C — min 61 HRC.
ENGINEERING NOTES
Weldability
Poor

D2 is not a structural welding grade — welding is limited to tool repair and edge build-up by experienced tool welders. Its high carbon and air-hardening response cause hard, crack-prone martensite in the heat-affected zone. Preheat to 250–400 °C and keep interpass temperature within the preheat range; use TIG for edge repair and SMAW for larger build-up. Cool slowly. Hardened tools: temper after welding at 10–20 °C below the original tempering temperature. Annealed material: re-anneal, then harden and temper the complete tool. Machine or grind the weld before final heat treatment where possible.

Filler metals
  • ER312 · AWS / TIG (GTAW)Buffer layer or crack-tolerant joining where weld hardness is not critical — not a wear-face deposit
  • E312-16 · AWS / SMAWStick equivalent of ER312 for buffer layers and repair of cracked tools
  • T Fe8 · EN 14700 / TIG (GTAW)Matching-hardness edge build-up for cold work tools, approx. 55–60 HRC as welded [VERIFY — confirm consumable brand/class with welding supplier]
  • E Fe8 · EN 14700 / SMAWStick electrode for larger cold work tool build-up, approx. 55–60 HRC as welded [VERIFY — confirm consumable brand/class with welding supplier]
Machinability
Fair

Machine in the soft annealed condition (≤255 HB) — machinability is roughly half that of plain carbon tool steel because of the hard primary chromium carbides. Use coated carbide tooling, rigid set-ups and moderate cutting speeds; HSS is suitable only for drilling and tapping at low speed. Leave a grinding allowance for heat-treatment size change. After hardening, finish by grinding with soft-grade, open-structure wheels and plenty of coolant to avoid grinding cracks. For wire EDM of hardened tools, use the high-temperature tempering route (≥500 °C) and re-temper after EDM to remove the brittle re-cast layer.

Applications

  • Blanking, piercing and trimming dies for high-volume sheet metal stamping
  • Punches and die buttons for long-run stamping of electrical steel laminations
  • Thread rolling dies and flat dies for stud, bolt and fastener production
  • Cold forming, coining and deep-drawing dies where abrasive wear limits tool life
  • Shear blades and slitting knives for steel service centres across the UAE and GCC
  • Granulator, pelletiser and shredder knives for plastics recycling and waste processing plants
  • Roll-forming rolls for steel profiles, purlins and cladding used in GCC construction
  • Cold extrusion dies and compaction punches for powder metallurgy parts
  • Wear-resistant mould inserts for glass-filled and mineral-filled engineering plastics
  • Woodworking, paper and packaging knives requiring long edge retention
  • Gauges, wear strips and precision fixtures needing dimensional stability after hardening

Related grades in Tool Steel

Frequently Asked Questions

Quick answers on our grades, certification, supply and lead times.

Still have questions?

Our team responds fast with specifications, certification and stock availability.

Contact our team

D2 tool steel is used for long-run cold work tooling where wear resistance decides tool life — blanking and piercing dies, punches, thread rolling dies, shear blades, slitting knives and cold forming dies. At 58–62 HRC its chromium carbides resist abrasion from sheet steel, electrical steel laminations and filled plastics far longer than low-alloy tool steels. In the UAE and GCC it is widely specified for stamping tools in automotive and appliance supply, shear blades in steel service centres, roll-forming rolls for construction profiles, and granulator knives in plastics recycling.

Get in touch

Elevateyourprojectswithoursuperiorsteel