Tool Steel dealers in UAE

S1 / 1.2550 / 60WCrV8 Shock-Resisting Tool Steel | Supplier in UAE & GCC

1.2550 / 60WCrV8 (S1 type) — tungsten-alloyed shock-resisting tool steel for chisels, heavy punches and shear blades that must take impact without chipping.

Industries Served

Manufacturing
Heavy Engineering
Construction
Automotive
Mould & Die

Overview

S1 / 1.2550 / 60WCrV8 is a tungsten-chromium-vanadium shock-resisting tool steel specified to EN ISO 4957, with AISI S1 (UNS T41901, ASTM A681) as its nearest US equivalent. It contains about 0.60% carbon, 2% tungsten, 1% chromium and 0.15% vanadium. Compared with high-carbon cold work steels, the lower carbon gives a tough martensite with few hard carbides. Tungsten and vanadium form fine carbides that refine the grain and add fatigue strength. Silicon supports tempering resistance. The result is a steel that takes repeated impact without chipping or cracking — the reason it is the standard choice for chisels and heavy punches. It is oil or warm-bath hardened from 860–900 °C and tempered at 180–300 °C for a working hardness of about 54–58 HRC. For moderate hot work it can be tempered at 550 °C or above. Note that ASTM A681 S1 runs lower in carbon (0.40–0.55%) and higher in chromium, so the two grades are close substitutes rather than identical. 1.2550 is supplied soft annealed to 229 HB maximum.

Nifty Alloys supplies S1 / 1.2550 / 60WCrV8 shock-resisting tool steel through our Dubai, UAE facility in round bar and flat bar, soft annealed and ready for machining and heat treatment. 1.2550 is supplied on request against your order to EN ISO 4957, with ASTM A681 S1 chemistry available where your drawing calls for it. For urgent cold work jobs, O1 / 1.2510 is held in Dubai stock. Every order carries an EN 10204 3.1 Mill Test Certificate as standard, confirming chemistry and annealed hardness with full traceability to the producing mill. EN 10204 3.2 third-party inspection is available on request. We deliver across the UAE and the GCC — Saudi Arabia, Kuwait, Qatar, Oman and Bahrain — and export to Europe, India and Africa. As an ISO 9001:2015 certified tool steel supplier in the UAE, our team can advise on shock-resisting steel selection for chisels, punches and blades. Contact our team to request a quote.

Chemical Composition

0.6 %
C

Carbon

0.55 – 0.65 %

Si

Silicon

0.7 – 1 %

Mn

Manganese

0.15 – 0.45 %

P

Phosphorus

≤ 0.03 %

S

Sulfur

≤ 0.03 %

1 %
Cr

Chromium

0.9 – 1.2 %

2 %
W

Tungsten

1.7 – 2.2 %

0.15 %
V

Vanadium

0.1 – 0.2 %

Mo

Molybdenum

Ni + Cu
Typical value Range (min–max) Minimum (≥) Maximum (≤) Hover / tap for notes

Standard

EN ISO 4957

EN

Revision: EN ISO 4957:2018

Tool steels — specification for chemical composition, heat treatment, and properties of tool steels including cold work, hot work, and high-speed grades.

Published as BS EN ISO 4957; leading BS dropped to match house style. European standard governing 1.2379 (X153CrMoV12) and other DIN tool steel grades. Supersedes former DIN 17350 for tool steels. Referenced in European and Middle Eastern engineering procurement. Equivalent German standard: DIN EN ISO 4957.

Available Forms

Round Bar

10–300 mm. Diameter. Typical mill range, supplied on request — confirm size and lead time at enquiry. [VERIFY with sales]

Flat Bar

10–150 mm. Thickness. Widths to order. Supplied on request. [VERIFY with sales]

Stock & delivery

Stock location
Dubai, UAE
In stock
Annealed — S1 / 1.2550 is supplied on request (not held as Dubai stock) to EN ISO 4957; ASTM A681 S1 on specific request. Lead time confirmed at quotation. O1 / 1.2510 annealed is held in Dubai stock as an alternative for less impact-critical tools.
Delivery UAE
24–48 hours
Delivery GCC
3–5 working days — Saudi Arabia, Kuwait, Qatar, Oman, Bahrain
Export
Europe, India, Africa on request
Quotation
Same-day quotation
Minimum order
No minimum order quantity for standard sizes

Key standards

EN ISO 4957

Designations & Equivalents

StandardDesignationNotes
AISI / SAES1Nearest US equivalent — ASTM A681 S1 chemistry differs from 1.2550 (lower C, higher Cr / V)
UNST41901UNS number for AISI S1 — nearest equivalent, not identical
EN / Werkstoff1.2550European material number — primary supply designation
DIN60WCrV8German / EN designation
DIN60WCrV7Former DIN 17350 name still used on drawings [VERIFY — source not confirmed]
EN Name60WCrV8EN ISO 4957 steel name
ISO60WCrV8ISO 4957 designation
ASTMA681 (S1)ASTM product standard for the nearest US type
BSBS1BS 4659 — withdrawn, legacy UK shock-resisting type [VERIFY — source not confirmed]
AMSNoneNo AMS specification applies to S1 / 1.2550 — not an aerospace procurement grade
Common NameShock-resisting tool steel, chisel steel, S1 tool steel, 2550 steelBuyer search terms used in UAE / GCC and Europe

Compliance & Certification

StandardStatusNotes
EN 10204 3.1SuitableMill Test Certificate provided as standard. Confirms chemistry and annealed hardness to EN ISO 4957 (or ASTM A681 S1 where ordered).
EN 10204 3.2ConditionalAvailable on request — specify at order stage. Additional lead time and cost may apply.

Specifications

Mechanical Properties

Values per EN ISO 4957. Bar length compares conditions within each row.

PropertyAnnealed | EN ISO 4957
Hardness (annealed)229 HBmaxSurface, as suppliedMax per EN ISO 4957 (one producer quotes 250 HB). ASTM A681 S1 max also 229 HB.
Tensile Strength (UTS)–Room tempNot specified by EN ISO 4957 for annealed tool steel — leave blank.
Yield Strength (0.2% Proof Stress)–Room tempNot specified — leave blank.
Elongation–Not specified — leave blank.
Hardness (hardened & tempered)56 HRCtypical860–900 °C oil + 200 °C temperTypical — producer data (54–58 HRC range). Not a specified value.
Impact Energy (Charpy)–No numeric data from producers — qualitative "high impact toughness". [VERIFY — source not confirmed]

Physical Properties

PropertyAnnealed | EN ISO 4957
Densityat 20°C–[VERIFY — source not confirmed]. Leave blank until confirmed.
Modulus of Elasticityat 20°C–[VERIFY — source not confirmed]. Leave blank until confirmed.
Thermal Conductivityat 20°C31.9 W/m·K
Coefficient of Thermal Expansionat 20–100°C10.9 µm/m·°C
Specific Heat Capacityat 20°C–[VERIFY — source not confirmed]. Leave blank until confirmed.
Melting Point / Rangeat Solidus–[VERIFY — source not confirmed]. Leave blank until confirmed.

Service Conditions

Service Temperature

Max 200 °C

Notes

For cold work — chisels, punches and shear blades tempered at 180–300 °C — the tool must work below its tempering temperature, so the working limit is about 200 °C. For moderate hot work, such as hot punching and gripper dies, temper at 550 °C or above; the tool then accepts brief contact with hot metal and water cooling in service, at a lower hardness. 1.2550 has only medium hot hardness — use 1.2714 or H13 / 1.2344 for sustained hot forging or die-casting tools.

Corrosion Performance

General corrosion

No corrosion resistance. 1.2550 rusts quickly in humid or coastal UAE and GCC conditions and in marine shipyard use. Store under cover with rust-preventive oil, and oil chisels and punches between uses. It is not a stainless steel.

Pitting resistance

No pitting resistance in chloride environments.

Additional notes

Not applicable — low-alloy tool steel (about 1% Cr).

Heat Treatment

ProcessTemperatureCoolingResult & notes
HEAT TREATMENT GUIDES1 / 1.2550 / 60WCrV8: Soft Annealing: 720–760 °Cabout 4 hslow furnace cooling — max 229 HB. Stress Relieving: 600–650 °C — about 2 h — slow furnace cooling. After heavy rough machining, before finish machining and hardening. Preheating: About 650 °C before hardening, especially for large or complex tools. Hardening: Austenitise at 860–900 °C — hold until through-heated plus soak — quench in oil, or in a warm bath at 180–220 °C for lowest distortion. Temper as soon as the tool is hand-warm. Tempering (cold work): 180–300 °C for a working hardness of about 54–58 HRC. Minimum 2 h, or 2 h per 25 mm section; air cool. Double tempering recommended. Typical hardness after tempering: 150 °C — 56–58 HRC; 200 °C — 54–58 HRC; 250 °C — 53–55 HRC; 350 °C — 51–53 HRC; 400 °C — 49–52 HRC. Tempering (hot work): 550 °C minimum for hot punching and gripper dies; tools may then be water-cooled in service. Hardening response (ASTM A681 S1 — only for material ordered to ASTM A681): preheat 677 °C, austenitise 941 °C (salt bath) or 954 °C (controlled atmosphere) for 5–15 min, oil quench, single 2 h temper at 204 °C — minimum 56 HRC. Forging: 1000–1050 °C; reheat if the bar falls below 900 °C; cool slowly, preferably in a furnace, then anneal. Post-weld Stress Relief (annealed material): 600–650 °C — furnace cooling.
ENGINEERING NOTES
Weldability
Poor

1.2550 is not used for welded joints — at about 0.6% carbon with W and Cr it hardens on cooling and the heat-affected zone cracks easily. Repair of chisels, punches and blades is possible with preheat, interpass held at or above preheat, low-hydrogen practice and slow cooling [VERIFY — preheat range to be confirmed from producer welding data]. Annealed material should be stress relieved at 600–650 °C after welding. Hardened tools must be re-tempered after repair. Ask us before repairing a hardened tool.

Filler metals
  • ER312 · AWS A5.9 / TIG (GTAW)Buffer (buttering) layer on crack-sensitive base metal before hard build-up. Not a matching-hardness deposit.
  • Shock-resisting matching rod, 52–58 HRC deposit · Tool-steel repair rod / TIG (GTAW)For edge build-up on chisels, punches and blades. [VERIFY — consumable code and classification to be confirmed with consumable supplier]
Machinability
Good

Machines well in the soft-annealed condition (≤229 HB) — its low carbide content makes it easier on cutting tools than 12% Cr cold work steels. Use coated carbide or HSS for turning and milling and HSS for drilling and tapping. Stress relieve at 600–650 °C after heavy rough machining and before finish machining. After hardening, grind with plenty of coolant to avoid softening the edge of chisels and blades.

Applications

  • Cold shear blades for cutting steel plate up to about 10 mm thick
  • Pneumatic chisels, rivet sets and air-hammer tools for GCC construction and shipyards
  • Heavy-duty piercing punches for thick plate in structural steel fabrication
  • Scrap and billet shear blades for metal recycling yards in the UAE
  • Paper, wood and plastics cutting knives that see impact or edge loading
  • Cold chisels, drifts, nail sets and hand tools for the trades
  • Gripper, forming and trimming dies under repeated shock
  • Solid and hollow embossing and marking punches
  • Mandrel bars for tube drawing and swaging dies
  • Ejector pins, tool holders and clutch parts needing toughness at 54–58 HRC
  • Moderate hot punching and gripper dies, tempered at 550 °C or above and water-cooled in service

Frequently Asked Questions

Quick answers on our grades, certification, supply and lead times.

Still have questions?

Our team responds fast with specifications, certification and stock availability.

Contact our team

S1 / 1.2550 tool steel is used for tools that must survive repeated impact without chipping or cracking. Typical parts are pneumatic and cold chisels, rivet sets, heavy piercing punches, shear blades for plate up to about 10 mm, scrap shear blades, embossing punches, gripper and trimming dies, and tube-drawing mandrels. Hardened and tempered to 54–58 HRC, its tough tungsten-alloyed martensite absorbs shock that would break high-carbon die steels. In the UAE and GCC it is used mainly by construction contractors, shipyards, steel fabricators and recycling yards.