Tool Steel dealers in UAE

1.2767 / 45NiCrMo16 / X45NiCrMo4 Tough Tool Steel | Supplier in UAE & GCC

1.2767 / 45NiCrMo16 — 4% Ni-Cr-Mo tough tool steel: through-hardens in large sections to 50–56 HRC, high toughness and polishability; dies, blades, moulds.

Industries Served

Mould & Die
Manufacturing
Automotive
Heavy Engineering

Overview

1.2767 (45NiCrMo16 to EN ISO 4957, formerly X45NiCrMo4, AISI ~6F7, French 45NCD16) is a nickel-chromium-molybdenum tool steel containing 0.40–0.50% carbon, 3.80–4.30% nickel, 1.20–1.50% chromium and 0.15–0.35% molybdenum. Its high nickel content gives exceptional toughness and through-hardenability: it can be hardened from 840–870°C in oil, air or a hot bath — even in large cross-sections — to 53–58 HRC, and is normally tempered to a working hardness of about 50–56 HRC. The result is a tool steel with very high resistance to bending, impact and cracking, high compressive strength and low distortion in heat treatment, combined with good polishability, etchability and erodibility. It is supplied soft annealed (285 HB maximum, typically 260 HB) for machining, or pre-hardened to about 40–44 HRC for tools used without further heat treatment. Typical applications are shear and scrap-shearing blades, cold heading and coining dies, bending tools, cutting and stamping tools for thick material, plastic moulds requiring a high polish, and heavy-duty components such as anvil blocks and rams.

Nifty Alloys supplies 1.2767 / 45NiCrMo16 tool steel to order from Dubai, UAE, in round bar, flat bar and plate / block, annealed as standard, with pre-hardened and ESR (electro-slag remelted) material on request. Every supply is dispatched with EN 10204 3.1 Mill Test Certificates as standard, certifying EN ISO 4957 chemistry, delivery condition and hardness with full traceability to the mill; EN 10204 3.2 third-party inspection is available on request. We deliver across the UAE, to Saudi Arabia, Kuwait, Qatar, Oman and Bahrain, and export to Europe, India and Africa, with lead time confirmed at quotation. Send your size list or drawing to request a quote — quotations are turned around the same day.

Chemical Composition

0.45 %
C

Carbon

0.4 – 0.5 %

0.25 %
Si

Silicon

0.1 – 0.4 %

0.4 %
Mn

Manganese

0.2 – 0.5 %

4 %
Ni

Nickel

3.8 – 4.3 %

1.35 %
Cr

Chromium

1.2 – 1.5 %

0.25 %
Mo

Molybdenum

0.15 – 0.35 %

P

Phosphorus

≤ 0.03 %

S

Sulfur

≤ 0.03 %

Typical value Range (min–max) Minimum (≥) Maximum (≤) Hover / tap for notes

Standard

EN ISO 4957

EN

Revision: EN ISO 4957 — current edition

Tool steels — specification for chemical composition, heat treatment, and properties of tool steels including cold work, hot work, and high-speed grades.

Published as BS EN ISO 4957; leading BS dropped to match house style. European standard governing 1.2379 (X153CrMoV12) and other DIN tool steel grades. Supersedes former DIN 17350 for tool steels. Referenced in European and Middle Eastern engineering procurement. Equivalent German standard: DIN EN ISO 4957.

Available Forms

Flat Bar

10–200 mm. Thickness; width to order.

Plate / Block

50–600 mm. Thickness of forged blocks; to order.

Round Bar

20–500 mm. Diameter, annealed; to order.

Stock & delivery

Stock location
Dubai, UAE (supplied to order)
In stock
Supplied to order — Annealed (+A) standard; Pre-Hardened 40–44 HRC and ESR on request.
Delivery UAE
Lead time confirmed at quotation
Delivery GCC
Lead time confirmed at quotation — Saudi Arabia, Kuwait, Qatar, Oman, Bahrain
Export
Europe, India, Africa on request
Quotation
Same-day quotation
Minimum order
No minimum order quantity; mill minimums may apply to special sizes

Key standards

EN ISO 4957

Designations & Equivalents

StandardDesignationNotes
EN / Werkstoff1.2767Material number — primary designation
EN Name45NiCrMo16EN ISO 4957 steel name
DINX45NiCrMo4Former DIN name
DINDIN 17350Superseded German tool-steel standard — legacy reference only
AISI / SAE6F7 — nearestCommonly quoted US equivalent
Common Name45NCD16(AFNOR) French designation
Common Name1.2767 ESR (electro-slag remelted variant)Premium cleanliness variant — supplied on request
Common NameTough tool steel / nickel tool steel / 2767 / shear blade steelBuyer search terms

Compliance & Certification

StandardStatusNotes
EN 10204 3.1SuitableProvided as standard — EN ISO 4957 chemistry, delivery condition and hardness.

Specifications

Mechanical Properties

Values per EN ISO 4957. Bar length compares conditions within each row.

PropertyAnnealed (+A) | EN ISO 4957Pre-Hardened 40–44 HRC | EN ISO 4957
Hardness285 HBmaxTypical 260 HBSoft annealed (+A)EN ISO 4957 maximum; typical as delivered ≤ 260 HB.40–44 HRCPre-hardened, as suppliedTypical producer range [VERIFY — confirm with supplying mill].
Hardness52 HRCminTest: 850°C oil, tempered 180°CEN ISO 4957 minimum hardening response.–
Hardness50–56 HRCWorking hardness after hardening and temperingTypical tool working range — guidance.–
Tensile Strength (UTS)880 MPatypicalAnnealedTypical — not specified.–

Physical Properties

PropertyAnnealed (+A) | EN ISO 4957Pre-Hardened 40–44 HRC | EN ISO 4957
Densityat 20°C7.85 g/cm³7.85 g/cm³
Thermal Conductivityat 20°C28 W/m·K28 W/m·K
Specific Heat Capacityat 20°C460 J/kg·K460 J/kg·K
Electrical Resistivityat 20°C0.3 µΩ·m0.3 µΩ·m

Service Conditions

Service Temperature

Notes

Service limit depends on the tempering temperature: keep tools at least about 50°C below the tempering temperature (producer guidance for plastic moulds) to avoid softening and distortion. Primarily a cold-work / tough tool steel; for sustained hot work use a hot-work grade such as H13 / 1.2344.

Corrosion Performance

General corrosion

Hardened tools are susceptible to stress-corrosion and hydrogen effects; temper immediately after hardening while the tool is at about 80°C, and avoid electroplating hardened edges without baking.

Pitting resistance

Not corrosion resistant. Moulds and tools rust in humid and coastal UAE and GCC conditions — keep oiled and store dry; for corrosive polymers specify a stainless mould steel.

Additional notes

Not applicable — not a stainless steel.

Heat Treatment

HEAT TREATMENT GUIDE — 1.2767 / 45NiCrMo16 / X45NiCrMo4

Hot forming: 1050–850°C. Soft annealing: 610–650°C for about 2–5 h, slow furnace cooling (10–20°C/h) to about 600°C, then air — 285 HB max (EN ISO 4957), typically ≤ 260 HB. Stress relieving: 600–650°C, about 4 h, slow furnace cooling — after rough machining. Hardening: preheat in steps (about 400°C and 650°C), then 840–870°C, hold 15–30 min after through-heating; quench in oil (interrupt at about 150°C), air, or hot bath at about 180–220°C — 53–58 HRC as quenched. EN ISO 4957 test: 850°C oil, temper 180°C → 52 HRC min. Tempering: immediately after quenching (tool at about 80°C), at least twice; 1 h per 20 mm, minimum 2 h — about 52 HRC at 250°C, falling with higher temperatures; working hardness typically 50–56 HRC. For moulds, temper at least 50°C above the operating temperature. Pre-hardened condition: producer-tempered to about 40–44 HRC [VERIFY]. ESR variant: for highest polish and homogeneity.

ENGINEERING NOTES
Weldability
Poor

Tool repair welding only, with a qualified procedure: preheat to about 300–350°C [VERIFY — preheat range per producer], use a matching tool-steel or nickel-bearing filler, keep interpass at preheat, cool slowly and temper immediately after welding about 30°C below the original tempering temperature. Weld in the annealed or hardened-and-tempered state according to the repair procedure; avoid welding near critical edges.

Filler metals
  • Matching 1.2767-type filler rod · Tool-steel repair / TIGFor die and blade repair; preheat and post-weld temper essential
  • ER100S-1 · AWS A5.28 / TIGNi-Mo high-strength wire for buttering or non-cutting areas
  • E312-16 · AWS A5.4 / SMAWAustenitic electrode for non-critical repairs and dissimilar joints
Machinability
Fair

Moderate machinability in the annealed condition (≤ 260–285 HB) with carbide tooling. Rough machine, stress relieve at about 600–650°C, finish-machine, then harden. Pre-hardened 40–44 HRC material is machined with hard-steel carbide grades. The grade is EDM-erodible, polishable to a mirror finish and suitable for photo-etching / texturing.

Applications

  • Shear blades and scrap-shearing knives for steel service centres
  • Billet shears and cold shear knives for thick material
  • Coining, embossing and cold hobbing dies
  • Bending tools, pressure bars and forming inserts
  • Cutting and stamping tools for heavy-gauge sheet
  • Plastic injection moulds needing a high polish or texture
  • Anvil blocks, rams and drop-hammer tooling
  • Drawing jaws and heavy-metal processing tools
  • Hot-pressing tools for light-metal processing
  • High-toughness tooling for GCC fabrication and recycling plants

Related grades in Tool Steel

Frequently Asked Questions

Quick answers on our grades, certification, supply and lead times.

Still have questions?

Our team responds fast with specifications, certification and stock availability.

Contact our team

1.2767 / 45NiCrMo16 is used for tools that need very high toughness and compressive strength: shear and scrap-shearing blades, billet shears, coining, embossing and cold hobbing dies, bending tools, stamping tools for thick material, plastic moulds requiring a high polish, and heavy items such as anvil blocks and rams. In the UAE and GCC it is used by steel service centres, recyclers and tool shops.

Get in touch