Overview

AISI 4130 alloy steel (UNS G41300, DIN/EN 25CrMo4, Werkstoff 1.7218, BS 708M25, JIS SCM430) is a chromium-molybdenum low-alloy steel containing 0.28–0.33% carbon, 0.80–1.10% chromium and 0.15–0.25% molybdenum, widely specified for oil and gas pressure-containing and downhole components. Chromium raises hardenability and tempering resistance, while molybdenum refines the tempered martensite, improves toughness and suppresses temper embrittlement at the high tempering temperatures needed for sour service. Its lower carbon gives 4130 better weldability than 4140, at the cost of shallower hardenability in heavy sections. For H2S service, 4130 is quenched and tempered to 80 ksi (552 MPa) minimum yield at a maximum of 22 HRC, meeting the NACE MR0175 / ISO 15156-2 limit for low-alloy steel; for sweet-service tools it is tempered lower to 110 ksi (758 MPa) minimum yield. Typical uses include wellhead and tree bodies, valve bodies, BOP components, subs, mandrels and downhole tool housings.

Nifty Alloys supplies AISI 4130 / 25CrMo4 from stock in Dubai, UAE, in quenched and tempered round bar, with open-die forgings, rings and seamless tube or hollow bar to ASTM A519 available to order. Sour-service material is supplied in the 80K NACE MR0175 condition with hardness verified at ≤22 HRC, and 110K yield material is available for non-sour downhole applications. Every delivery is certified to EN 10204 3.1, confirming chemistry, mechanical properties and full heat traceability; EN 10204 3.2 third-party inspection is available on request. We deliver within the UAE in 24–48 hours and across the GCC to Saudi Arabia, Kuwait, Qatar, Oman and Bahrain, with export to Europe, India and Africa on request. Contact our team to request a quote — same-day turnaround with current stock sizes confirmed.

Chemical Composition

0.3 %
C

Carbon

0.28 – 0.33 %

0.25 %
Si

Silicon

0.15 – 0.35 %

0.5 %
Mn

Manganese

0.4 – 0.6 %

0.95 %
Cr

Chromium

0.8 – 1.1 %

0.2 %
Mo

Molybdenum

0.15 – 0.25 %

P

Phosphorus

≤ 0.035 %

S

Sulfur

≤ 0.04 %

Ni

Nickel

≤ 0.25 %

Cu

Copper

≤ 0.35 %

Fe

Iron

Typical value Range (min–max) Minimum (≥) Maximum (≤) Hover / tap for notes

Standard

ASTM A29 / A29M

ASTM

Revision: ASTM A29/A29M — current edition; NACE MR0175 / ISO 15156-2:2020 (revision at FDIS stage Oct 2026 — update on publication)

Standard Specification for General Requirements for Hot-Wrought Steel Bars, Carbon and Alloy. Defines the chemical composition of AISI/SAE 4130 (UNS G41300) and the residual element limits.

Chemistry standard only — it does not set mechanical properties. 80K / 110K oil & gas properties are set by the purchase specification. Related ASTM product standards: A322 (alloy steel bars), A331 (cold-finished bars), A519 (seamless mechanical tubing).

Available Forms

Forging / Ring Forging

100–1500 mm. OD / largest dimension, to drawing; subject to forge capacity and Q&T section limits. [VERIFY]

Round Bar

20–500 mm. Diameter. Q&T 80K / 110K. Above ~250 mm, confirm test location (T/4 or mid-radius) — core properties depend on section. Cut to length. [VERIFY stock sizes]

Seamless Tube / Hollow Bar

40–400 mm. Outside diameter; wall thickness to order, ASTM A519. [VERIFY]

Stock & delivery

Stock location
Dubai, UAE
In stock
Q&T 80K NACE MR0175 (≤22 HRC) round bar — stock. 110K Q&T, forgings and seamless tube / hollow bar — on request. [CONFIRM against current stock list]
Delivery UAE
24–48 hours
Delivery GCC
3–5 working days — Saudi Arabia, Kuwait, Qatar, Oman, Bahrain
Export
Europe, India, Africa on request
Quotation
Same-day quotation
Minimum order
No minimum order quantity for standard sizes

Key standards

ASTM A29 / A29M

Designations & Equivalents

StandardDesignationNotes
AISI / SAE4130Primary designation
UNSG41300Unified Numbering System
EN / Werkstoff1.7218European material number for 25CrMo4 — close equivalent; chemistry not identical to 4130
DIN25CrMo4DIN 17200 designation (superseded by EN 10083-3)
EN Name25CrMo4EN 10083-3 / EN 10250-3
BS708M25BS 970 equivalent (also 708A25). [VERIFY — confirm against current BS 970 edition]
JISSCM430JIS G4053 — close equivalent
ISO25CrMo4ISO 683-2
ASTMA29 / A519 / A788Bar chemistry / seamless mechanical tube / forgings
AMSAMS 6348 / AMS 6370Aerospace bar and forging specifications — not covered by the SpecSheets on this page
Common Name25CD4AFNOR (France) designation
Common NameChromoly / Chrome Moly / CrMo steel / 4130 80K / 4130 NACETrade and buyer search terms

Compliance & Certification

StandardStatusNotes
EN 10204 3.1SuitableMill Test Certificate provided as standard with every delivery.
EN 10204 3.2ConditionalAvailable on request — specify at order stage; additional lead time and cost may apply.
NACE MR0175 / ISO 15156ConditionalCompliant only in the 80K Q&T condition: ≤22 HRC (≤237 HBW), Ni <1%, quenched and tempered, per ISO 15156-2 Annex A. The 110K condition (28–32 HRC) exceeds the limit and is not supplied as NACE-compliant solid bar. Welds require PWHT with hardness ≤250 HV10. Hardness results reported on the 3.1 certificate.
NACE MR0103 / ISO 17945ConditionalRefinery sour service — 80K Q&T condition at ≤22 HRC only.
API Spec 6AConditional80K material meets the API 6A 75K tensile requirements. PSL, temperature class and Charpy requirements must be stated at enquiry; PSL 3/4 adds hardness, NDE and traceability requirements.

Specifications

Mechanical Properties

Values per ASTM A29 / A29M. Bar length compares conditions within each row.

PropertyQ&T 80K NACE MR0175 (≤22 HRC) | ASTM A29Q&T 110K Yield (Non-Sour) | ASTM A29
Tensile Strength (UTS)655 MPaminTypical 720 MPaRoom temp, longitudinal, T/4 or mid-radius95 ksi min (purchase-spec minimum); typical value indicative862 MPaminTypical 930 MPaRoom temp, longitudinal, T/4 or mid-radius125 ksi min (purchase-spec minimum); typical value indicative
Yield Strength (0.2% Proof Stress)552 MPaminTypical 600 MPaRoom temp, longitudinal, T/4 or mid-radius80 ksi min; exceeds API 6A 75K (517 MPa)758–965 MPaTypical 820 MPaRoom temp, longitudinal, T/4 or mid-radius110–140 ksi range per common producer specifications
Elongation18 %minTypical 22 %50 mm gauge lengthPurchase-spec minimum; API 6A 75K requires 17%. [VERIFY vs customer spec]13 %minTypical 16 %50 mm gauge lengthProducer-spec minimum. [VERIFY vs customer spec]
Reduction of Area35 %minTypical 55 %LongitudinalAPI 6A 75K minimum; typical value indicative40 %minTypical 50 %Longitudinal[VERIFY — source not confirmed]
Hardness22 HRCmaxTypical 20 HRCSurface and section surveyNACE MR0175 / ISO 15156-2 maximum; ≤237 HBW30 HRCtypicalSurfaceTypically 28–32 HRC; set by yield requirement. Exceeds NACE 22 HRC limit
Impact Energy (Charpy)–V-notch, per ordered temperature classPer customer spec / API 6A temperature class (typically −29°C or −46°C). [VERIFY — enter value when PO specifies]–V-notch, per ordered temperaturePer customer spec. [VERIFY — enter value when PO specifies]

Physical Properties

PropertyQ&T 80K NACE MR0175 (≤22 HRC) | ASTM A29Q&T 110K Yield (Non-Sour) | ASTM A29
Densityat 20°C7.85 g/cm³7.85 g/cm³
Modulus of Elasticityat 25°C205 GPa205 GPa
Thermal Conductivityat 100°C42.7 W/m·K42.7 W/m·K
Coefficient of Thermal Expansionat 20–100°C12.2 µm/m·°C12.2 µm/m·°C
Specific Heat Capacityat 20°C477 J/kg·K477 J/kg·K
Melting Point / Rangeat Solidus1432 °C1432 °C

Service Conditions

Service Temperature

Max 400 °C

Notes

Minimum service temperature is set by the Charpy test temperature ordered — typically −29°C or −46°C for API 6A temperature classes — so it is left blank rather than stated as a grade property. Upper limit of about 400°C reflects loss of tensile strength and onset of creep in tempered Cr-Mo steel; long service above this needs code-based allowable stresses (e.g. 1.25Cr-0.5Mo grades). Service temperature must always stay well below the final tempering temperature. In sour service, the environment and API 6A temperature class (up to 121°C for class U) govern before strength does.

Corrosion Performance

General corrosion

Rusts in humid and coastal atmospheres; GCC storage needs oil or VCI protection. In sour service the risk is cracking (SSC, HIC), governed by hardness and microstructure rather than metal loss — hence the 22 HRC limit. CO2-dominated wells need inhibition or CRA weld overlay (e.g. Alloy 625) on 4130 bodies.

Pitting resistance

No meaningful pitting resistance. Pits and corrodes in seawater and chloride brines — coat, clad or select a corrosion-resistant alloy for wetted surfaces.

Additional notes

Not applicable — low-alloy steel.

Heat Treatment

ProcessTemperatureCoolingResult & notes
HEAT TREATMENT GUIDEAISI 4130 / 25CrMo4 / 708M25 Forging: 1200°C maximum start, finish above 950°C; slow cool after forging. Normalising: 870–900°Chold 1 h per 25 mmair cool. Refines grain before Q&T; standard pre-treatment for forgings. Annealing: 845–870°C — hold 1 h per 25 mm — furnace cool at ≤20°C/h to 650°C, then air cool. Typical 150–180 HBW for machining. [VERIFY typical hardness] Hardening: 855–885°C — soak minimum 1 h, plus 30 min per 25 mm — water or polymer quench for sections over ~25 mm; oil for thin sections to limit distortion and cracking. As-quenched 48–52 HRC at the surface. Tempering — 80K NACE: typically 650–690°C — minimum 1 h per 25 mm — air cool. Target ≤22 HRC (≤237 HBW) with 80 ksi (552 MPa) minimum yield. Tempering — 110K: typically 540–600°C — minimum 1 h per 25 mm — air cool. Target 28–32 HRC with 110 ksi (758 MPa) minimum yield. Avoid tempering between 260°C and 370°C (tempered-martensite embrittlement). Stress relieving: 600–650°C and at least 30°C below the last tempering temperature — 1 h per 25 mm — slow cool. Section size: 4130 is shallow-hardening. Rough-machine forgings before Q&T, use a vigorous quench, and test at T/4 or mid-radius or on a qualification test coupon per API 6A. Core properties of very large sections will be lower than at T/4.
ENGINEERING NOTES
Weldability
Good

Weldable with a qualified low-hydrogen procedure; carbon equivalent (IIW) is typically about 0.60, so hydrogen control is essential. Use H4 or H8 consumables, preheat 150–260°C rising with thickness and restraint (minimum 200°C above 25 mm), and keep interpass at or above preheat, maximum 315°C. Post-weld heat treat Q&T material at 620–675°C, at least 25–30°C below the base-metal tempering temperature. PWHT is mandatory for NACE MR0175 service, where weld metal and HAZ must not exceed 250 HV10 and filler metals must contain less than 1% Ni. 110K material needs its own qualified procedure — a PWHT low enough to protect its strength may not adequately temper the HAZ.

Filler metals
  • ER80S-D2 · AWS A5.28 / GTAW-GMAWMn-Mo wire, Ni ≤0.15%. Matches 80K strength after PWHT; acceptable for sour service.
  • ER80S-B2 · AWS A5.28 / GTAW-GMAW1.25Cr-0.5Mo wire — closest Cr-Mo chemistry match. PWHT required.
  • E8018-B2-H4 · AWS A5.5 / SMAWLow-hydrogen 1.25Cr-0.5Mo electrode, Ni <1%. Sour-service capable.
  • E10018-D2-H4 · AWS A5.5 / SMAWHigher-strength Mn-Mo electrode for 110K non-sour joints; verify strength after PWHT.
Machinability
Good

Machinability is about 70% of AISI 1212 in the annealed / cold-drawn condition. In the 80K NACE condition (≤22 HRC) 4130 machines well with coated carbide (ISO P15–P25). 110K material at 28–32 HRC needs rigid set-ups, P20–P30 carbide and reduced cutting speeds. On NACE parts, cold work that raises surface hardness above 22 HRC must be followed by stress relief per ISO 15156-2 — confirm against the project specification.

Applications

  • API 6A wellhead, tree and tubing-head bodies to 75K material designation for sour service
  • Gate and ball valve bodies, bonnets and end connections for H2S-containing production lines
  • BOP components, drilling spools and adapter flanges for well-control equipment
  • Downhole tool housings, mandrels and sleeves machined from 4130 hollow bar
  • Drill-string subs, crossovers and pup joints in 110K yield for non-sour wells
  • Choke bodies and manifold blocks for wellhead and production manifolds in GCC fields
  • Forged rings, hubs and flanges for subsea and topside connectors
  • Swivels, plug valves and flow-iron components for well-service and frac equipment
  • Hydraulic cylinder bodies and pressure-containing parts for offshore cranes and handling gear

Related grades in Alloy Steel

Frequently Asked Questions

Quick answers on our grades, certification, supply and lead times.

Still have questions?

Our team responds fast with specifications, certification and stock availability.

Contact our team

AISI 4130 is used mainly for oil and gas pressure-containing and downhole components — wellhead and tree bodies, valve bodies, BOP parts, manifolds, subs and tool housings — where strength, toughness and weldability are needed together. In the UAE and GCC, most 4130 is bought in the 80K NACE MR0175 condition (≤22 HRC) for sour-service wellhead and valve equipment, while 110K yield material is used for sweet-service downhole tools. Outside oil and gas, 4130 is used for hydraulic cylinder bodies, forged rings and flanges, offshore handling equipment and, in normalised form, welded aircraft and motorsport tubing.

Get in touch