EN40B / 722M24 / EN40BT Nitriding Steel | Supplier in UAE & GCC

EN40B / 722M24 / EN40BT — 3% Cr-Mo nitriding steel: 850–1000 MPa Condition T core, 750 HV min nitrided case with minimal distortion; shafts, gears.

Industries Served

Automotive
Aerospace & Defence
Heavy Engineering
Manufacturing
Oil & Gas

Overview

EN40B (BS 970 722M24, supplied pre-hardened as EN40BT / 722M24T, aerospace BS S106) is a 3% chromium-molybdenum nitriding steel containing 0.20–0.28% carbon, about 3.0–3.5% chromium and 0.45–0.65% molybdenum. The high chromium content forms hard, stable chromium nitrides during gas or plasma nitriding, giving a surface hardness of at least about 750 HV (roughly 62 HRC) while molybdenum resists temper embrittlement during the long nitriding cycle. Because nitriding is carried out at a relatively low temperature, below the tempering temperature, there is no quench — components emerge scale-free with minimal distortion, and the case adds compressive stress that improves fatigue strength. The steel is supplied hardened and tempered to Condition T (850–1000 MPa, 248–302 HB), which provides a tough, high-strength core and is readily machinable before nitriding; it also offers good creep strength for elevated-temperature service. EN40B is used for crankshafts, camshafts, gears, spindles, pump shafts, hydraulic rods and precision components where wear resistance and dimensional stability matter. There is no exact EN equivalent; 31CrMo12 (EN 10085) is the nearest.

Nifty Alloys supplies EN40B / 722M24 nitriding steel from stock in Dubai, UAE, in round bar, hardened and tempered to Condition T as standard, with annealed material and Conditions S or U on request. Bars are cut to length and dispatched with EN 10204 3.1 Mill Test Certificates as standard, certifying 722M24 chemistry, condition, tensile, impact and hardness results with full traceability to the mill; EN 10204 3.2 third-party inspection is available on request. We deliver across the UAE within 24–48 hours, to Saudi Arabia, Kuwait, Qatar, Oman and Bahrain within 3–5 working days, and export to Europe, India and Africa. Send your size list or drawing to request a quote — quotations are turned around the same day.

Chemical Composition

0.24 %
C

Carbon

0.2 – 0.28 %

Si

Silicon

0.1 – 0.35 %

Mn

Manganese

0.45 – 0.7 %

3.25 %
Cr

Chromium

3 – 3.5 %

0.55 %
Mo

Molybdenum

0.45 – 0.65 %

Ni

Nickel

≤ 0.4 %

P

Phosphorus

≤ 0.035 %

S

Sulfur

≤ 0.04 %

Typical value Range (min–max) Minimum (≥) Maximum (≤) Hover / tap for notes

Standard

BS 970-1 (withdrawn)

Other

Revision: BS 970-1:1996 (withdrawn — legacy specification)

Available Forms

Round Bar

16–250 mm. Diameter, Condition T; precision ground on request. Condition T properties subject to ruling section. [VERIFY — stock range not confirmed]

Stock & delivery

Stock location
Dubai, UAE
In stock
H&T Condition T (EN40BT) — standard stocked condition. Conditions S / U and annealed on request. Nitriding by the customer.
Delivery UAE
24–48 hours
Delivery GCC
3–5 working days — Saudi Arabia, Kuwait, Qatar, Oman, Bahrain
Export
Europe, India, Africa on request
Quotation
Same-day quotation
Minimum order
No minimum order quantity for standard sizes

Key standards

BS 970-1 (withdrawn)

Designations & Equivalents

StandardDesignationNotes
BSEN40B / EN40BTOriginal BS 970:1955 designation; T = Condition T (850–1000 MPa)
BS722M24 / 722M24TBS 970 designation (withdrawn standard) — governing chemistry
Common NameBS S106(BS Aerospace) UK aerospace equivalent of 722M24 — aliases only
EN Name31CrMo12 / 1.8515 — nearest only(EN (nearest)) EN 10085 nitriding steel; higher carbon (0.28–0.35%) — not an exact equivalent
DIN32CrMo12 / 1.7361 — nearest onlyFormer DIN designation often quoted — not an exact equivalent
Common Name30CD12(AFNOR) French designation (nearest)
Common NameEN40B nitriding steel / 3% chrome moly steel / nitriding steel round bar / EN40BTBuyer search terms

Compliance & Certification

StandardStatusNotes
EN 10204 3.1SuitableProvided as standard — 722M24 chemistry, condition, tensile, impact and hardness.
EN 10204 3.2ConditionalAvailable on request with independent third-party inspection — specify at order stage.
NACE MR0175 / ISO 15156Not Applicable — Not a sour-service grade: Condition T (248–302 HB) and the nitrided case exceed the 22 HRC limit for low-alloy steels.

Specifications

Mechanical Properties

Values per BS 970-1 (withdrawn). Bar length compares conditions within each row.

PropertyH&T Condition T | BS 970-1Annealed | BS 970-1
Tensile Strength (UTS)850–1000 MPaCondition TBS 970 722M24 range.–
Yield Strength (0.2% Proof Stress)680 MPaminCondition TPublished minimum (some sources: 650 MPa).–
Elongation13 %minA (5.65√So)Published minimum.–
Impact Energy (Charpy V-notch)50 JminRoom temp, KCVPublished value (some sources: 35 J).–
Hardness248–302 HBCondition TBS 970 range.–AnnealedMaximum reported on MTC [VERIFY — annealed hardness limit not confirmed].
Hardness750 HVminNitrided surfaceGuidance — achievable after gas / plasma nitriding (700–850 HV typical).–

Physical Properties

PropertyH&T Condition T | BS 970-1Annealed | BS 970-1
Densityat 20°C7.85 g/cm³7.85 g/cm³
Modulus of Elasticityat 20°C205 GPa205 GPa
Thermal Conductivityat 20°C35 W/m·K35 W/m·K
Coefficient of Thermal Expansionat 20–100°C12 µm/m·°C12 µm/m·°C

Service Conditions

Service Temperature

Max 500 °C

Notes

[VERIFY — maxServiceTempC 500: continuous load-bearing limit not confirmed] In Condition T the steel offers high creep strength, with producers quoting use up to about 600°C for some applications; nitrided parts should stay below the nitriding temperature (about 500–530°C) to preserve the case. Not for cryogenic service without impact testing.

Corrosion Performance

General corrosion

Unprotected Condition T bar rusts in humid, coastal UAE and GCC conditions — store oiled. Nitrided rods are used as an alternative to hard chrome plating in hydraulic service.

Pitting resistance

Base metal has no pitting resistance. The nitrided compound layer gives moderately improved resistance to atmospheric corrosion and mild chemical attack compared with bare steel.

Additional notes

Not applicable — low-alloy steel (3% Cr is not enough for passivity).

Heat Treatment

HEAT TREATMENT GUIDE — EN40B / 722M24 / EN40BT

Forging: preheat carefully, forge at 850–1200°C, do not forge below 850°C; cool slowly in still air. Softening / annealing: heat slowly to 680–700°C, cool in air. Hardening: about 880–910°C — quench in oil. Tempering: 570–700°C, air cool — Condition T 850–1000 MPa (248–302 HB). Temper above the planned nitriding temperature so the core is stable during nitriding. Stress relieving: after rough machining, below the tempering temperature, before finish machining and nitriding. Nitriding: gas nitriding at about 500–530°C (or plasma / salt-bath), duration set by required case depth — surface about 750 HV minimum (approximately 62 HRC; 700–850 HV typical). No quench needed; minimal distortion and very small growth. Re-hardening: re-harden and re-temper only before nitriding — heating nitrided parts above the nitriding temperature degrades the case.

ENGINEERING NOTES
Weldability
Poor

Welding is not recommended: 3% chromium with molybdenum gives high hardenability and a crack-prone HAZ. If unavoidable, weld before nitriding with preheat, low-hydrogen Cr-Mo consumables, controlled interpass temperature and post-weld heat treatment [VERIFY — procedure parameters not confirmed]. Never weld nitrided surfaces — the nitrided case cracks and the nitrogen causes porosity.

Filler metals
  • E9018-B3 · AWS A5.5 / SMAW2.25Cr-1Mo low-hydrogen electrode — nearest Cr-Mo match for repairs before nitriding
  • ER90S-B3 · AWS A5.28 / TIG / MIG2.25Cr-1Mo wire for GTAW / GMAW; preheat and PWHT required
  • E309L-16 · AWS A5.4 / SMAWAustenitic electrode for non-load-bearing attachments where PWHT is impossible
Machinability
Good

Readily machinable in Condition T (248–302 HB) with carbide tooling. Complete all machining, then stress relieve below the tempering temperature, finish-grind and nitride — growth during nitriding is very small, so parts can be finished close to size. After nitriding only light grinding or lapping is practical.

Applications

  • Nitrided crankshafts for motorsport and high-performance engines
  • Camshafts, cam followers and valve-train components
  • Gears, pinions and gear wheels needing low-distortion surface hardening
  • Spindles, quills and precision machine-tool shafts
  • Pump shafts and seal sleeves for GCC process and water pumps
  • Nitrided hydraulic cylinder rods and pistons as a hard-chrome alternative
  • Gudgeon pins, bushes and guide pins
  • Aerospace components to BS S106
  • Extrusion and injection-moulding screws and barrels
  • Bolts and fixings requiring wear-resistant threads

Frequently Asked Questions

Quick answers on our grades, certification, supply and lead times.

Still have questions?

Our team responds fast with specifications, certification and stock availability.

Contact our team

EN40B / 722M24 is used for nitrided components that need a very hard, wear-resistant surface with minimal distortion: crankshafts, camshafts, gears, spindles, pump shafts, hydraulic cylinder rods, gudgeon pins and extrusion screws. After nitriding the surface reaches at least about 750 HV over a tough 850–1000 MPa core. In the UAE and GCC it is used for pump shafts, hydraulic rods and precision machinery parts.

Get in touch

Elevateyourprojectswithoursuperiorsteel