Alloy Steel dealers in UAE

EN31 / 535A99 / 100Cr6 / 52100 Bearing Steel | Supplier in UAE & GCC

EN31 / 100Cr6 / 52100 — 1% C, 1.5% Cr through-hardening bearing steel: 207 HB max annealed, about 62 HRC hardened; bearings, rollers, gauges, punches.

Industries Served

Automotive
Manufacturing
Mould & Die
Heavy Engineering
Aerospace & Defence

Overview

EN31 (BS 970 535A99, 100Cr6 / 1.3505 to EN ISO 683-17, AISI 52100 to ASTM A295, JIS SUJ2, GB GCr15) is a high-carbon chromium through-hardening steel and the world's standard ball and roller bearing steel. Its 0.93–1.05% carbon and 1.35–1.60% chromium form fine, hard chromium carbides in a high-carbon martensite, giving a surface hardness of about 60–64 HRC after oil hardening from 830–870°C and tempering at 150–180°C, with high compressive strength, wear resistance and rolling-contact fatigue life. Bearing-quality 100Cr6 and 52100 add tight phosphorus and sulphur limits and controlled non-metallic inclusions, which govern fatigue life in bearings; the older BS 970 535A99 / EN31 designation allows wider manganese and chromium ranges and carries no cleanliness requirements. The steel is supplied spheroidised annealed (207 HB maximum) for machining and through-hardens fully in sections up to about 25–30 mm. Applications include bearing balls, rollers and rings, gauges, ejector pins, taps, punches, swaging dies and wear parts. BS 970 is withdrawn; 100Cr6 is the current European designation.

Nifty Alloys supplies EN31 / 100Cr6 / 52100 bearing steel from stock in Dubai, UAE, in round bar, spheroidised annealed as standard, with hardened and tempered material on request. Bars are cut to length and dispatched with EN 10204 3.1 Mill Test Certificates as standard, certifying chemistry (100Cr6, 52100 or 535A99 as supplied), delivery condition and hardness with full traceability to the mill; EN 10204 3.2 third-party inspection is available on request. We deliver across the UAE within 24–48 hours, to Saudi Arabia, Kuwait, Qatar, Oman and Bahrain within 3–5 working days, and export to Europe, India and Africa. Send your size list or drawing to request a quote — quotations are turned around the same day.

Chemical Composition

1 %
C

Carbon

0.93 – 1.05 %

Si

Silicon

0.15 – 0.35 %

Mn

Manganese

0.25 – 0.45 %

1.5 %
Cr

Chromium

1.35 – 1.6 %

Mo

Molybdenum

≤ 0.1 %

P

Phosphorus

≤ 0.025 %

S

Sulfur

≤ 0.015 %

Cu

Copper

≤ 0.3 %

Al

Aluminium

≤ 0.05 %

Typical value Range (min–max) Minimum (≥) Maximum (≤) Hover / tap for notes

Standard

EN ISO 683-17

EN

Revision: EN ISO 683-17 — current edition

Heat-treatable steels, alloy steels and free-cutting steels — Part 17: Ball and roller bearing steels. Covers 100Cr6 (1.3505) with bearing-quality cleanliness, chemistry and delivery-condition hardness requirements.

Primary standard for 100Cr6. Delivery conditions include spheroidised annealed (+AC, 207 HB max) and spheroidised annealed and cold drawn (+AC+C, 241 HB max). Includes non-metallic inclusion and microstructure requirements that general engineering grades do not.

Available Forms

Round Bar

6–100 mm. Diameter, spheroidised annealed; black, peeled or bright drawn. Larger sizes on request. [VERIFY — minimum stock size not confirmed]

Stock & delivery

Stock location
Dubai, UAE
In stock
Spheroidised Annealed (+AC, 207 HB max) — standard stocked condition. Hardened & Tempered on request.
Delivery UAE
24–48 hours
Delivery GCC
3–5 working days — Saudi Arabia, Kuwait, Qatar, Oman, Bahrain
Export
Europe, India, Africa on request
Quotation
Same-day quotation
Minimum order
No minimum order quantity for standard sizes

Key standards

EN ISO 683-17

Designations & Equivalents

StandardDesignationNotes
BSEN31Original BS 970:1955 designation — primary buyer term
BS535A99BS 970 designation (withdrawn standard) — wider Mn / Cr, general-engineering quality
EN Name100Cr6EN ISO 683-17 bearing steel — primary chemistry on this page
EN / Werkstoff1.3505100Cr6 material number (bearing steel)
AISI / SAE52100 / E52100ASTM A295 bearing steel
UNSG52986Unified Numbering System for E52100
AMSAMS 6440 [VERIFY — Ashwin to confirm]52100 aircraft-quality bars, forgings and tubing — aliases only
AMSAMS 6444 [VERIFY — Ashwin to confirm]52100 consumable-electrode vacuum-remelted (premium) quality — aliases only
JISSUJ2Japanese Industrial Standard
Common NameGCr15(GB) Chinese designation
Common Name100C6 / 2258(AFNOR / SS) French and Swedish designations
Common Name1.2067 (102Cr6)(Not equivalent) Tool-steel grade of similar chemistry without bearing-quality requirements — NOT the same material as 1.3505
Common NameEN31 round bar / bearing steel / chrome steel / ball bearing steel / 52100 steelBuyer search terms

Compliance & Certification

StandardStatusNotes
EN 10204 3.1SuitableProvided as standard — chemistry (100Cr6, 52100 or 535A99 as supplied), delivery condition and hardness.
EN 10204 3.2ConditionalAvailable on request with independent third-party inspection — specify at order stage.
NACE MR0175 / ISO 15156Not Applicable — Not a sour-service grade: hardened bearing steel at about 60–64 HRC far exceeds the 22 HRC limit for low-alloy steels.

Specifications

Mechanical Properties

Values per EN ISO 683-17. Bar length compares conditions within each row.

PropertySpheroidised Annealed (+AC) | EN ISO 683-17Hardened & Tempered | EN ISO 683-17
Hardness207 HBmaxSpheroidised annealed (+AC)EN ISO 683-17 maximum.60–64 HRCTypical 62 HRCOil hardened 830–870°C, tempered 150–180°CTypical range — process dependent.
Hardness241 HBmaxSpheroidised annealed + cold drawn (+AC+C)EN ISO 683-17 maximum.–
Hardness60–64 HRCAfter hardening 830–870°C oil + tempering 150–180°CAchievable hardness — guidance only.–
Tensile Strength (UTS)700 MPatypicalSpheroidised annealedTypical — not specified.2300 MPatypicalMartensitic, low-temperature temperTypical — not specified.
Yield Strength (0.2% Proof Stress)410 MPatypicalSpheroidised annealedTypical — not specified.1700 MPatypicalMartensitic, low-temperature temperTypical — not specified.
Elongation27 %typicalSpheroidised annealedTypical — not specified.2 %typicalMartensitic, low-temperature temperTypical — very low ductility.

Physical Properties

PropertySpheroidised Annealed (+AC) | EN ISO 683-17Hardened & Tempered | EN ISO 683-17
Densityat 20°C7.81 g/cm³7.81 g/cm³
Modulus of Elasticityat 20°C210 GPa210 GPa
Thermal Conductivityat 20°C42 W/m·K42 W/m·K
Coefficient of Thermal Expansionat 20–100°C11.4 µm/m·°C11.4 µm/m·°C

Service Conditions

Service Temperature

Max 150 °C

Notes

Hardened bearing steel tempered at 150–180°C loses hardness and dimensional stability if operated above its tempering temperature; standard bearings are generally limited to about 120–150°C. For higher service temperatures, components are tempered higher (with lower hardness) or a dimensionally stabilised heat treatment is specified. Toughness is low at sub-zero temperatures in the fully hardened condition.

Corrosion Performance

General corrosion

Corrodes like other low-alloy steels. Hardened parts (60–64 HRC) are highly susceptible to hydrogen embrittlement — avoid acid pickling and electroplating, or bake immediately after.

Pitting resistance

No corrosion resistance. Hardened bearing surfaces pit and lose fatigue life quickly in humid or coastal conditions typical of the UAE and GCC. Keep oiled or greased; for corrosive environments specify a stainless bearing steel such as 440C.

Additional notes

Not applicable — low-alloy steel (1.5% Cr is not enough for passivity).

Heat Treatment

HEAT TREATMENT GUIDE — EN31 / 100Cr6 / 1.3505 / 52100

Forging / hot rolling: 1100–850°C; cool slowly. Normalising: 870–900°C, air cool (to break up carbide networks before spheroidising). Soft / spheroidise annealing: about 780–800°C, slow furnace cool — 207 HB max (+AC); 241 HB max if subsequently cold drawn (+AC+C). Stress relief: 600–650°C, furnace cool, after rough machining and before final hardening. Hardening: 830–870°C in oil or polymer (800–830°C in water for small simple parts). Temper within 2 h. Tempering: 150–180°C, air cool — about 62–64 HRC (150°C ≈ 63 HRC, 200°C ≈ 62 HRC; higher tempering lowers hardness: 300°C ≈ 57 HRC). Hardenability: through-hardens in sections up to about 25–30 mm (rings up to about 17 mm wall in oil); larger sections develop a softer core. Sub-zero treatment: optional after quench to reduce retained austenite and improve dimensional stability for precision bearings and gauges.

ENGINEERING NOTES
Weldability
Poor

Welding is not recommended. About 1% carbon with 1.5% chromium makes the weld and heat-affected zone form brittle, high-carbon martensite that cracks readily, even with preheat. Join bearing-steel parts mechanically or by shrink fit; where an unavoidable repair is attempted on annealed material, use high preheat, controlled slow cooling and re-heat-treat the whole part.

Filler metals
  • E312-16 · AWS A5.4 / SMAWAustenitic stainless electrode for non-load-bearing repairs on annealed material only — dilution-tolerant
  • E7018 · AWS A5.1 / SMAWLow-hydrogen electrode for attaching non-critical fixtures to annealed bar only, with high preheat
Machinability
Fair

Machine in the spheroidised annealed condition (207 HB max) with carbide or HSS tooling and generous coolant — the spheroidised carbides give good chip control and finish. Leave grinding allowance for hardening distortion. After hardening (about 60–64 HRC) only grinding, hard turning or EDM is practical.

Applications

  • Ball and roller bearing balls, rollers and rings
  • Bearing races and sleeves for gearboxes and machine tools
  • Precision gauges, plug gauges and measuring tools
  • Ejector pins, guide pins and bushes for injection moulds
  • Punches, swaging dies and press tooling for light-duty cold work
  • Taps, thread rolls and small cutting tools
  • Cam followers, rollers and linear-motion shafts
  • Spindles and wear parts in GCC manufacturing and maintenance shops
  • Collets, chuck jaws and work-holding components
  • Pump plungers and valve components needing high surface hardness

Related grades in Alloy Steel

Frequently Asked Questions

Quick answers on our grades, certification, supply and lead times.

Still have questions?

Our team responds fast with specifications, certification and stock availability.

Contact our team

EN31 / 100Cr6 / 52100 is used for ball and roller bearing balls, rollers and rings, and for other parts that need very high surface hardness and wear resistance: precision gauges, ejector and guide pins, punches, swaging dies, taps, cam followers and pump plungers. Hardened and tempered it reaches about 60–64 HRC. In the UAE and GCC it is widely used by maintenance shops, mould makers and precision engineering workshops.

Get in touch

Elevateyourprojectswithoursuperiorsteel